[{"content":"Setting of cement paste is an important property to be measured. So how to measure it? The most common method is using Vicat needle instrument. The European Standards and ASTM both document the detailed method. One of the deferences of the two methods lies on the treatment of the surface of sample.\nThe \u0026ldquo;Methods of testing cement — Part 3: Determination of setting times and soundness\u0026rdquo; says \u0026ldquo;Place the filled mould and base-plate in the container, add water so that the surface of the paste is submerged to a depth of at least 5 mm, and store in the temperature controlled enclosure at (20,0 ± 1,0) °C\u0026rdquo;.\nWhile the ASTM \u0026ldquo;C191 − 13 Standard Test Methods for Time of Setting of Hydraulic Cement by Vicat Needle\u0026rdquo; shows that \u0026ldquo;Immediately after molding, place the test specimen in the moist cabinet or moist room and allow it to remain there except when penetration measurements are being made.\u0026rdquo;\nWe could see the point here is trying to keep the constant water to cement ratio of the surface of the sample, otherwise the dried surface would make trouble for the penetrating of the needle and give fake setting time point.\nHowever, it is difficult to apply European Standards to measure the setting of alkali activated cement paste. As the alkali ions dissolve into the water and significantly change the chemistry of the surface layer. If there is no moist curing cabinet, how can we test the setting of alkali activated cement paste?\nHere we share the trick that we have been using at our lab with you. Use Vaseline (petroleum jelly)! After pouring the paste into the mould, cover the surface with a thin layer of melting Vaseline (about 100 °C), the Vaseline is then immediately cooled into a layer of gel.\nWhy choose Vaseline instead of water?\nThe Vaseline is easy to be melted and cover the surface and soon returns to soft gel status. The soft gel functions as the water layer preventing the surface losing water due to drying. What is more, the Vaseline does not have chemical reaction with alkali activated cement, nor do the alkali ions dissolve into Vaseline. And the price of Vaseline is cheap. So ladies use Vaseline for makeup, we use it for cement research.\n","permalink":"https://www.cementscience.com/2015/04/use-vaseline-to-cover-the-surface-of-alkali-activated-cement-paste-during-setting-test.html","summary":"\u003cp\u003eSetting of cement paste is an important property to be measured. So how to measure it? The most common method is using Vicat needle instrument. The European Standards and ASTM both document the detailed method. One of the deferences of the two methods lies on the treatment of the surface of sample.\u003c/p\u003e\n\u003cp\u003eThe \u0026ldquo;Methods of testing cement — Part 3: Determination of setting times and soundness\u0026rdquo; says \u0026ldquo;Place the filled mould and base-plate in the container, add water so that the surface of the paste is submerged to a depth of at least 5 mm, and store in the temperature controlled enclosure at (20,0 ± 1,0) °C\u0026rdquo;.\u003c/p\u003e","title":"Use Vaseline to cover the surface of alkali activated cement paste during setting test"},{"content":"In the previous post, I introduced the protocol to measure the yield stress of cement paste. I would like to share the method how to measure the plastic viscosity of cement paste.\nThe principle determine the plastic viscosity of cement paste is using the relationship between shear rate and shear stress. Applying a serials of shear rate on the cement paste would result in the corresponding shear stress. After obtaining the set of shear rate and shear stress, the plastic viscosity of the paste is calculated by regression.\nThe measured shear rate and shear stress of a cement paste, Measuring device: HAAKE™ VT550 (ViscoTester VT550), CR (Controlled shear Rate): 0-100 1/s; t 120.00 s; T 20.00 °C.\nThe paste should be measured by increasing shear rate and then the decreasing rate. Typical shear rate applied on cement paste is linearly between 0 and 100 1/s. Since the rheological feature of most of cement pastes is a kind of Bingham model, we can choose the liner part of the decreasing shear curve from the date set (shear rate vs. shear stress) for the regression. The slope from the regression equation is the so-called plastic viscosity.\nHowever, if the rheological cure of the paste behaves rather than Bingham model, selecting an appropriate model is necessary.\n","permalink":"https://www.cementscience.com/2015/03/the-method-to-measure-the-plastic-viscosity-of-cement-paste.html","summary":"\u003cp\u003eIn the previous post, I introduced the \u003ca href=\"https://www.cementscience.com/2015/02/the-right-protocol-to-measure-yield-stress-of-cement-paste.html\"\u003eprotocol to measure the yield stress\u003c/a\u003e of cement paste. I would like to share the method how to measure the plastic viscosity of cement paste.\u003c/p\u003e\n\u003cp\u003eThe principle determine the plastic viscosity of cement paste is using the relationship between shear rate and shear stress. Applying a serials of shear rate on the cement paste would result in the corresponding shear stress. After obtaining the set of shear rate and shear stress, the plastic viscosity of the paste is calculated by regression.\u003c/p\u003e","title":"The method to measure the plastic viscosity of cement paste"},{"content":"The rheology of cementitious material paste is complex and difficult to be investigated. One value of rheology is yield stress. The best method to measure the yield stress in laboratory is using the vane method. However, there is no much literature reporting an practical and detailed testing protocol to measure the yield stress of cement paste. Here I briefly introduce the protocol I am using at our laboratory.\nTo obtain stable and reliable results, we should choose the same container and the same mixing procedure. We normally use a plastic beaker with a volume 500 ml, for the beaker has enough diameter and depth for the test without the influence of boundary effect, i.e. the diameter is two times larger than the diameter of the vane. For each test, 270 g of cement is mixed with relevant water at the required water to cement ratio. For the mixing, a high-shear mixer is applied with a shear rate 800 RPM for 2 minutes.\nAs soon as the well mixed paste is ready, let the blades of the vane of rheometer immerse in the paste. Make sure the top surface of the paste staying between the two lines labeled on the shaft.\nThe principle to measure the yield stress is applying a very low fixed shear rate on the paste, e.g 0.02-0.001 1/s, then the shear stress linearly increases till yield stress. As shown in the recorded data (Fig 1), the shear stress drops remarkably when the paste is yield, thus the maximum stress is the yield stress, i.e. dynamic yield stress.\nFig. 1. Measuring device: HAAKE™ VT550 (ViscoTester VT550), CR (Controlled shear Rate): 0.01000 1/s; t 120.00 s; T 20.00 °C.\nIf the maximum stress does not occur within the testing period, longer time or higher shear rate may be tried. It is also worth to note that this method gives good result for paste with yield stress higher than 10 Pa.\n","permalink":"https://www.cementscience.com/2015/02/the-right-protocol-to-measure-yield-stress-of-cement-paste.html","summary":"\u003cp\u003eThe rheology of cementitious material paste is complex and difficult to be investigated. One value of rheology is yield stress. The best method to measure the yield stress in laboratory is using the vane method. However, there is no much literature reporting an practical and detailed testing protocol to measure the yield stress of cement paste. Here I briefly introduce the protocol I am using at our laboratory.\u003c/p\u003e\n\u003cp\u003eTo obtain stable and reliable results, we should choose the same container and the same mixing procedure. We normally use a plastic beaker with a volume 500 ml, for the beaker has enough diameter and depth for the test without the influence of boundary effect, i.e. the diameter is two times larger than the diameter of the vane. For each test, 270 g of cement is mixed with relevant water at the required water to cement ratio. For the mixing, a high-shear mixer is applied with a shear rate 800 RPM for 2 minutes.\u003c/p\u003e","title":"The right protocol to measure yield stress of cement paste"},{"content":"Particle size is a very important property in the research field of cementitious materials, e.g. modeling, reaction kinetics.\nParticles are 3-dimensional objects, and unless they are perfect spheres, e.g. emulsions or bubbles, they cannot be fully described by a single dimension such as a radius or diameter.\nIn order to simplify the measurement process, it is often convenient to define the particle size using the concept of equivalent spheres. In this case the particle size is defined by the diameter of an equivalent sphere having the same property as the actual particle such as volume or mass for example.\nIt is important to realize that different measurement techniques use different equivalent sphere models and therefore will not necessarily give exactly the same result for the particle diameter.\nBelow is a schematic figure illustrating the definition of particle size based on different equivalent spheres.\nDefinition of particle size\n","permalink":"https://www.cementscience.com/2015/01/how-to-define-particle-size.html","summary":"\u003cp\u003eParticle size is a very important property in the research field of cementitious materials, e.g. modeling, reaction kinetics.\u003c/p\u003e\n\u003cp\u003e\u003ca href=\"http://www.atascientific.com.au/publications/wp-content/uploads/2012/07/MRK1806-01-basic-guide-to-particle-characterisation.pdf\"\u003eParticles are 3-dimensional objects\u003c/a\u003e, and unless they are perfect spheres, e.g. emulsions or bubbles, they cannot be fully described by a single dimension such as a radius or diameter.\u003c/p\u003e\n\u003cp\u003eIn order to simplify the measurement process, it is often convenient to define the particle size using the concept of equivalent spheres. In this case the particle size is defined by the diameter of an equivalent sphere having the same property as the actual particle such as volume or mass for example.\u003c/p\u003e","title":"How to define particle size?"},{"content":"I have been confused by the term \u0026ldquo;Geopolymer cement (concrete)\u0026rdquo; for long time. Some researchers told me Geopolymer cement is essentially alkali activated cement/material (AAMs), such as alkali activated slag and fly ash. Since alkali activated slag is indeed a kind of geopolymer cement, it looks logical to consider Geopolymer cement as alkali activated cement.\nIs it correct? Recently, I read the State of the Art report on alkali activated cement (Alkali Activated Materials State-of-the-Art Report, RILEM TC 224-AAM), finding the description:\nLow-calcium alkali-activated systems, predominantly dealing with alkali aluminosilicates and including those materials which are now widely known as ‘geopolymers’.\nIt is clear that not all alkali activated cements are geopolymers. Just those with low calcium materials activated by alkali in cement industry are regarded as geopolymer cement, in other words, geopolymers are shown here as a subset of AAMs, with the highest Al and lowest Ca concentrations.\nBTW, Davidovits is the first researcher applied the name ‘geopolymer’ to these low calcium materials activated by alkali. He was working in France, patented numerous aluminosilicate-based formulations for niche applications from the early 1980s onwards.\n","permalink":"https://www.cementscience.com/2014/12/what-is-geopolymer-cement.html","summary":"\u003cp\u003eI have been confused by the term \u0026ldquo;Geopolymer cement (concrete)\u0026rdquo; for long time. Some researchers told me Geopolymer cement is essentially alkali activated cement/material (AAMs), such as alkali activated slag and fly ash. Since alkali activated slag is indeed a kind of geopolymer cement, it looks logical to consider Geopolymer cement as alkali activated cement.\u003c/p\u003e\n\u003cp\u003eIs it correct? Recently, I read the State of the Art report on alkali activated cement (Alkali Activated Materials State-of-the-Art Report, RILEM TC 224-AAM), finding the description:\u003c/p\u003e","title":"What is Geopolymer cement?"},{"content":"Authors: Zhijun Tan, Geert De Schutter, Guang Ye, Yun Gao, Lieven Machiels\nAbstract:\nThis paper investigates the influence of slag particle size on its hydration speed at particle level in the early age. Slags were separated with sieves into groups of different size fractions, considering a wide range of sizes. The chemical compositions of each group were analyzed by X-ray Fluorescence (XRF). Activated by 15% Ca(OH)2 (by mass) at water/powder ratio 1:1, the hydration heat evolution was recorded by isothermal calorimetry up to 84 hours and converted to hydration degree. Based on the hydration degrees and particle size distributions, the rate of increase of hydrating layer thickness of each single slag particle (k value) was calculated. Results reveal that k values of coarse particles are higher than that of fine particles. Coarse particles contain higher content of CaO but relatively lower content of MgO, Al2O3 and SiO2, resulting in higher reactivity index of (CaO+Al2O3+MgO)/SiO2.\nKeywords: Blast-furnace slag, Particle size distribution, Reactivity, Hydration degree\nFull paper link.\n","permalink":"https://www.cementscience.com/2014/02/influence-of-particle-size-on-the-early-hydration-of-slag-particle-activated-by-caoh2-solution.html","summary":"\u003cp\u003eAuthors: Zhijun Tan, Geert De Schutter, Guang Ye, Yun Gao, Lieven Machiels\u003c/p\u003e\n\u003cp\u003eAbstract:\u003c/p\u003e\n\u003cp\u003eThis paper investigates the influence of slag particle size on its hydration speed at particle level in the early age. Slags were separated with sieves into groups of different size fractions, considering a wide range of sizes. The chemical compositions of each group were analyzed by X-ray Fluorescence (XRF). Activated by 15% Ca(OH)\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e (by mass) at water/powder ratio 1:1, the hydration heat evolution was recorded by isothermal calorimetry up to 84 hours and converted to hydration degree. Based on the hydration degrees and particle size distributions, the rate of increase of hydrating layer thickness of each single slag particle (k value) was calculated. Results reveal that k values of coarse particles are higher than that of fine particles. Coarse particles contain higher content of CaO but relatively lower content of MgO, Al\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003eO\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003e and SiO\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e, resulting in higher reactivity index of (CaO+Al\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003eO\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003e+MgO)/SiO\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e.\u003c/p\u003e","title":"Influence of Particle Size on the Early Hydration of Slag Particle Activated by Ca(OH)2 Solution"},{"content":"It is well known that cement is the most used construction material in the world. In the mind of most of people, cement is a kind of grey powder and only used as construction material, to build gardens, bridges, road etc. However, we can do more with cement, here are nice pictures showing some stuff made of cement. Creactive!\nEven as a guy like me who deals with cement everyday, I really think these items are pretty funny. What do you think you can do using cement? make the most of your imagination, dare to think.\n","permalink":"https://www.cementscience.com/2013/08/what-can-you-do-using-cement-funny-stuff-made-of-cement.html","summary":"\u003cp\u003eIt is well known that cement is the most used construction material in the world. In the mind of most of people, cement is a kind of grey powder and only used as construction material, to build gardens, bridges, road etc. However, we can do more with cement, here are nice pictures showing some stuff made of cement. Creactive!\u003c/p\u003e\n\u003cp\u003eEven as a guy like me who deals with cement everyday, I really think these items are pretty funny. What do you think you can do using cement? make the most of your imagination, dare to think.\u003c/p\u003e","title":"What can you do using cement? Funny stuff made of cement"},{"content":"These following conclusions are summarized from the work of Kocaba\u0026rsquo;s PhD thesis.\nalite: no influence is shown on the consumption of alite measured by XRD. belite: the substitution of cement by both slags seems to result in a delay in the hydration of belite in the first days. aluminate phase: there is a filler effect using inert filler at about 12 hours of hydration, which shows slag can also has filler effect in the early hydration period. Transformation of AFt to AFm causes cumulative heat shoulder at about 60 hours. For all systems, slags did not have a strong influence on hydration of C3A phases. Taking into account the low content of C3A and the corresponding error, it was difficult to highlight any relevant difference between blended paste and corresponding pure pastes.\nThere was no evidence of slag itself reacting and the effect of slag on aluminate phases can be only attributed to a filler effect.\nThe raw calorimetry curves of pure cement system showed a peak (called IV) which was attributed to monosulfoaluminate reaction just around 60 hours of reaction. In this way, calcium hemicarboaluminate and monocarboaluminate could be some possible AFm phases corresponding to the second peak of aluminate. But there is no evidence of that and it could be some monosulfate. The corresponding XRD patterns did not show any peaks corresponding to AFm phases at early ages which indicate a very low content if they are present.\nFerite: The slags seem to favour the hydration of the ferrite phase. Influence of slag on the degree of reaction of cement\nFrom XRD-Rietveld refinement and SEM-IA, the degree of reaction of cement did not seem to be strongly affected by the slag.\n","permalink":"https://www.cementscience.com/2013/07/the-influence-of-slag-on-the-hydration-of-cement.html","summary":"\u003cp\u003eThese following conclusions are summarized from the work of Kocaba\u0026rsquo;s PhD thesis.\u003c/p\u003e\n\u003cul\u003e\n\u003cli\u003e\u003cstrong\u003ealite\u003c/strong\u003e: no influence is shown on the consumption of alite measured by XRD.\u003c/li\u003e\n\u003cli\u003e\u003cstrong\u003ebelite\u003c/strong\u003e: the substitution of cement by both slags seems to result in a delay in the hydration of belite in the first days.\u003c/li\u003e\n\u003cli\u003e\u003cstrong\u003ealuminate phase\u003c/strong\u003e: there is a filler effect using inert filler at about 12 hours of hydration, which shows slag can also has filler effect in the early hydration period. Transformation of AFt to AFm causes cumulative heat shoulder at about 60 hours.\u003c/li\u003e\n\u003c/ul\u003e\n\u003cblockquote\u003e\n\u003cp\u003eFor all systems, slags did not have a strong influence on hydration of C3A phases. Taking into account the low content of C3A and the corresponding error, it was difficult to highlight any relevant difference between blended paste and corresponding pure pastes.\u003c/p\u003e\n\u003cp\u003eThere was no evidence of slag itself reacting and the effect of slag on aluminate phases can be only attributed to a filler effect.\u003c/p\u003e\n\u003cp\u003eThe raw calorimetry curves of pure cement system showed a peak (called IV) which was attributed to monosulfoaluminate reaction just around 60 hours of reaction. In this way, calcium hemicarboaluminate and monocarboaluminate could be some possible AFm phases corresponding to the second peak of aluminate. But there is no evidence of that and it could be some monosulfate. The corresponding XRD patterns did not show any peaks corresponding to AFm phases at early ages which indicate a very low content if they are present.\u003c/p\u003e\n\u003c/blockquote\u003e","title":"The Influence of Slag on the Hydration of Cement"},{"content":"Concrete is the most used material in the world because of its cheap price and large quantity. It is needless to say concrete is made of cement. However, cement is also a criticized material by the public, for its intensive CO2 emission from production process. The production of cement accounts for about 5-8% of the non-natural CO2 worldwide.\nPeople may ask, can we find an alternative construction material instead of cement? such as wood, steel. The annual usage of wood is much above the replanting level, and it is not possible to get wood in some places such as Africa and China. As for steel, it is costly and again the production of steel also gives CO2 emission. Furthermore, the production of cement is not that energy intensive compared with other materials.\nActually, it is not possible to find an alternative construction material. 98% of the earth’s crust is made of eight elements: O, Si, Al, Fe, Ca, Na, K, Mg, which are the main elements of cement as well. From the long term run, the world will still need a large amount of cement. The demand of cement mainly comes from developing countries, such as India and China because of the urbanization and its population growth.\nSince we have to use cement in the future, how can we do to reduce the CO2 emission and what is the future of cement? Efforts have been doing ever since decades ago in the cement industry and research community.\nOn the one hand, cement plants nowadays burn (hazardous) waste, say, car tyres, as fuel to make cement. The wood floating on the water of Three Gorges Dam is even collected to make fuel for cement plants. On the other hand, the production process of cement has always been optimizing. Some cement plants can even reach 80% efficiency, which is a great achievement even from a theoretical standpoint.\nResearchers of cement try to use less cement clinkers. One viable method is Supplementary Cementitious Materials (SCMs). SCMs are commonly industry by-products or raw materials, such as Slag, limestone, Fly ash, silica fume, natural pozzolan. Whether binary blended or even ternary blended, SCMs can replace part of cement without sacrificing equivalent engineering properties.\nConsidering the limited quantity and access of SCMs, SCMs are not a permanent sustainable way from a long term run. Some researchers are trying to utilize the unlimited amount of calcined clay, for the kaolinite content of clay has similar cementitious property. Work done replacing 30% of cement by calcined clay in Cuba shows the potential future of clay if well used.\nGenerally speaking, cement is a significantly important construction material, and it is not necessary to worry that much as for the CO2 emission in the future.\n","permalink":"https://www.cementscience.com/2013/06/the-importance-of-cement-and-its-future.html","summary":"\u003cp\u003eConcrete is the most used material in the world because of its cheap price and large quantity. It is needless to say concrete is made of cement. However, cement is also a criticized material by the public, for its intensive CO\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e emission from production process. The production of cement accounts for about 5-8% of the non-natural CO\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e worldwide.\u003c/p\u003e","title":"The Importance of Cement and its Future"},{"content":"What is Buoyancy Effect of TGA experiment?\nTGA (thermogravimetric analysis) is an important method to analyze the hydration products of cementitious materials. When a TGA test for cementitious materials sample is performed, the initial TGA curve may appears as such:\nA typical TGA test result shows the buoyancy effect. Portland cement past, w/c=0.4, cured 1 day.\nAs can be seen from the curve, the mass exceeded the original mass, which is not reasonable, since the decomposition of the sample always decrease the mass of testing sample. So why does this happen? This is because of the buoyancy effect in the TGA equipment.\nEvery substance found in a gas atmosphere is subjected to a buoyant force. This results in \u0026ldquo;apparent\u0026rdquo; mass changes. The degree of buoyancy, and thus the degree of mass change as well, are basically dependent on the volume of the substance and the density of the prevailing gas.\nHowever, for thermogravimetric investigations, it is not the absolute value of the buoyancy at a certain temperature that is decisive, but rather its change as a function of temperature. A typical buoyancy curve is shown as follows.\nA blank TGA test.\nIt was recorded using a NETZSCH STA 409 with a DSC sample carrier in a static N2 atmosphere. There is no sample in the crucible, but the recorded result shows the mass is always over ZERO.\nDue to the volume-dependence of the buoyancy, it is important to specify the sample carrier type in addition to the gas atmosphere, since different sample carrier/crucible combinations give rise to different \u0026ldquo;apparent\u0026rdquo; mass changes.\nHow to remove the Buoyancy Effect?\nKnowing this, we can remove the buoyancy effect by running a blank test. Repeat the test with the same crucible but without anything in it or with inert material, then the buoyancy effect is recorded. Subtracting the buoyancy result from the first measurement result, the true mass change of the test is obtained.\nA typical TGA test result after the subtracted the blank test, removing the buoyancy effect. Portland cement past, w/c=0.4, cured 1 day.\nWhy does the buoyancy curve initially show such a drastic rise?\nYou may find the buoyancy curve initially shows a drastic rise, why is that? This phenomenon arises from the design of TGA device.\nAt low temperatures, heat transfer from the furnace to the sample thermocouple is exclusively through convection. Since a certain amount of time is required before the crucible material is evenly heated and the warm air preferably flows along the inside of the protective tube, and thus does not reach the crucible immediately, the actual temperature of the gas atmosphere is far higher, particularly at the beginning of a measurement, than the temperature sensor indicates. Therefore, the gas density changes dramatically in the beginning of the test, thus subjects dramatic “apparent mass” change.\nA schematic figure showing the temperature difference.\n","permalink":"https://www.cementscience.com/2013/04/buoyancy-effect-of-tga-experiment.html","summary":"\u003cp\u003e\u003cstrong\u003eWhat is Buoyancy Effect of TGA experiment?\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eTGA (thermogravimetric analysis) is an important method to analyze the hydration products of cementitious materials. When a TGA test for cementitious materials sample is performed, the initial TGA curve may appears as such:\u003c/p\u003e\n\u003cp\u003e\u003cimg alt=\"A typical TGA test result. Portland cement past, w/c=0.4, cured 1 day. \" loading=\"lazy\" src=\"/wp-content/uploads/2013/04/PC1D.jpg\"\u003e\u003c/p\u003e\n\u003cp\u003eA typical TGA test result shows the buoyancy effect. Portland cement past, w/c=0.4, cured 1 day.\u003c/p\u003e\n\u003cp\u003eAs can be seen from the curve, the mass exceeded the original mass, which is not reasonable, since the decomposition of the sample always decrease the mass of testing sample. So why does this happen? This is because of the buoyancy effect in the TGA equipment.\u003c/p\u003e","title":"Buoyancy Effect of TGA Experiment"},{"content":"In the last post, I explained the clear definition of different densities. Among these densities, bulk density and apparent density are the two most important values when performing mercury intrusion porosity (MIP) experiment.\nSince samples that undergo MIP are usually irregular, the bulk volume is not possible to measure without being immersed in liquid. By the help of MIP, the bulk volume can be measured, thus the bulk density can be calculated simply dividing the mass by bulk volume.\nAt the end of MIP, the intruded volume of mercury at corresponding pressure is recorded, which means the pore volume is known. As soon as the bulk volume and pore volume are known, the solid volume including closed fine pores is also known. Then the porosity and apparent density are easily calculated.\nThe density of cement particles is commonly referred as 3.1 g/cm^3, and that of slag and limestone are 2.6 and 2.7 g/cm^3, respectively. You may be curious to know how about the bulk density of cement paste. Are they higher and lower than the raw materials? Are they stable values as curing ages extend and thus more hydration products formed?\nRecently, several cement and blended paste samples of mine have been tested using MIP. I list the bulk density results as below. All the pastes are mixed at water : powder = 0.4, sealed and cured at 20 °C. As each scheduled curing age (1, 3, 7, 14, 28 and 91 days) reaches, the hydration were stopped by liquid nitrogen, and later freeze dried to remove the frozen free water.\nBulk density of hydrating (blended) cement pastes.\nFrom the results, the bulk density of cement or blended cement ranges between 1.4 to 1.8 g/cm^3, much lower than raw material, and blended cement paste, such as the ternary blended cement paste, constantly has lower bulk density. This show that the hydrating blended cement pastes are more porous, which are further confirmed by tested porosity results below.\nPorosity of hydrating (blended) cement pastes.\n","permalink":"https://www.cementscience.com/2013/03/how-much-is-the-bulk-density-of-hydrating-blended-cement-paste.html","summary":"\u003cp\u003eIn the last post, I explained \u003ca href=\"https://www.cementscience.com/2013/03/what-is-density-how-to-distinguish-different-density-definitions.html\"\u003ethe clear definition of different densities\u003c/a\u003e. Among these densities, bulk density and apparent density are the two most important values when performing mercury intrusion porosity (MIP) experiment.\u003c/p\u003e\n\u003cp\u003eSince samples that undergo MIP are usually irregular, the bulk volume is not possible to measure without being immersed in liquid. By the help of MIP, the bulk volume can be measured, thus the bulk density can be calculated simply dividing the mass by bulk volume.\u003c/p\u003e","title":"How much is the bulk density of hydrating (blended) cement paste?"},{"content":"As material researchers, we know density is the physical property of materials. Even since grade school, we are taught that density is simply the mass of an object divided by its volume.\nHowever, this is pretty complicated in the case of cementitious materials. The mass of a certain amount of harden cement (or concrete) paste is a finite value, but how about the volume? since the harden cement paste is porous, how do we consider the open and close pores inside the paste as we want to determine the volume?\nI met the problem when I performed Mercury Intrusion Porosimetry (MIP) test, especially when I read the output result from the MIP machine, there are bulk density, skeletal density, envelope density and apparent density.\nIt is not difficult to find these definitions from either textbooks or internet. First I list them below:\nApparent particle density: The mass of a particle divided by its apparent (particle) volume (BSI).\nBulk density: (also called Bulk powder density): The apparent powder density under defined conditions.\nThe mass of the particles divided by the volume they occupy that includes the space between the particles (ASTM D5004).\nThe ratio of the mass of a collection of discrete pieces of solid material to the sum of the volumes of: the solids in each piece, the voids within the pieces, and the voids among the pieces of the particular collection (ASTM D3766).\nEnvelope density: The ratio of the mass of a particle to the sum of the volumes of: the solid in each piece and the voids within each piece, that is, within close-fitting imaginary envelopes completely surrounding each piece (ASTM D3766). The ratio of the mass of a particle to the envelope volume of the particle (implied by BSI).\nSkeletal density: The ratio of the mass of discrete pieces of solid material to the sum of the volumes of: the solid material in the pieces and closed (or blind) pores within the pieces (ASTM D3766).\nTrue density (also called True particle density): The mass of a particle divided by its volume, excluding open pores and closed pores (BSI).\nIt is a headache to me to well understand them and distinguish these different density definitions. I guess it is still not clear for people to understand these densities either. Fortunately, I found a schematic picture (below) well illustrate the physical meaning of these density definitions, which you may no longer misunderstand them any more.\nIs it now clear?\n","permalink":"https://www.cementscience.com/2013/03/what-is-density-how-to-distinguish-different-density-definitions.html","summary":"\u003cp\u003eAs material researchers, we know density is the physical property of materials. Even since grade school, we are taught that density is simply the mass of an object divided by its volume.\u003c/p\u003e\n\u003cp\u003eHowever, this is pretty complicated in the case of cementitious materials. The mass of a certain amount of harden cement (or concrete) paste is a finite value, but how about the volume? since the harden cement paste is porous, how do we consider the open and close pores inside the paste as we want to determine the volume?\u003c/p\u003e","title":"What is density? how to distinguish different density definitions?"},{"content":"Theoretical background: see chapters 3 and 4 in Lieven Machiels\u0026rsquo;s PhD thesis (2010). Sample preparation method modified from Machiels et al. (2008).\nRepresentative sampling\nThe mineralogy and glass content of slags depend largely on the mode of cooling of the slags, e.g. slow cooling in a slag pot can result in a large amount of crystalline phases, and fast granulation in water can result in high glass content. A mineralogical analysis will thus only represent the mineralogy of a slag system for a certain grade of cooling and strongly different results can be obtained when cooling conditions are different between the different batches.\nEven in a single slag pot, mineralogy and glass content can vary strongly. Taking a sample representative for a slag pot can be done by performing the sampling after a first size reduction of the bulk material or, by mixing representative parts of the slag pot (sides of the pot, center, near cracks, in center of slags, etc.)\nCrushing\nA grain size of \u0026lt;10 micron is required for quantitative X-ray diffraction (Rietveld). To avoid amorphisation of the sample during grinding, wet milling is done in a McCrone Micronizing mill. Before grinding in the McCrone Mill, the samples are crushed and passed through a 500 micron sieve.\nTake representative amounts of sample (50-100 g). Crush the sample by hand in a porcelain mortar. Use shock impact for grinding, avoid shearing. A jaw crusher can be used, but automatic milling devices which could induce shear stress of amorphisation such as ball mills should be avoided!\nMicronizing of the sample\nWeigh 2.7 g of sample; add 0.3 g (10%) of ZnO internal standard. Note down the exact weights, they will be used in the calculations\nMicronize the samples in a MeCrone Micronizing mill using 5 ml of ethanol (methanol) as grinding agent and a grinding time of 5 minutes for soft material (e. g. limestones) up to 10 minutes for hard materials (eg. quartzites, slags). Since methanol tends to react with some artificial minerals, and as it is toxic, ethanol is preferred. To ensure that samples are ground up to \u0026lt; 10 micron, the size required for X-ray quantification, the grain size is best checked by (wet) laser diffractometry.\nAfter micronizing, recuperate the sample in porcelain cups. Cover the cups with plastic foil, because recovery of powder from the porcelain when dried is difficult. Wash with methanol to recuperate as much as possible of the sample.\nDry for one—two days under a fume hood (methanol is toxic).\nPreparation for X-ray diffraction\nDried samples are gently disaggregated in an agate mortar and passed through a 250 micron sieve, to ensure good mixing of sample and ZnO standard.\n+/- 0.5 g of sample is needed for the X-ray analysis. Side-loading with frosted glass is recommended to fill sample holders, to prevent preferential orientation of fibrous zeolites and clay minerals. Sample holders are gently tapped while filling, to ensure good packing of the grains. Alternatively, back loading is used.\nThe content is offered by Dr. Lieven Machiels\n","permalink":"https://www.cementscience.com/2013/01/sample-preparation-for-quantitative-x-ray-diffraction-xrdrietveld.html","summary":"\u003cp\u003eTheoretical background: see chapters 3 and 4 in Lieven Machiels\u0026rsquo;s PhD thesis (2010). Sample preparation method modified from Machiels et al. (2008).\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003eRepresentative sampling\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eThe mineralogy and glass content of slags depend largely on the mode of cooling of the slags, e.g. slow cooling in a slag pot can result in a large amount of crystalline phases, and fast granulation in water can result in high glass content. A mineralogical analysis will thus only represent the mineralogy of a slag system for a certain grade of cooling and strongly different results can be obtained when cooling conditions are different between the different batches.\u003c/p\u003e","title":"Sample Preparation for Quantitative X-Ray Diffraction (XRD/Rietveld)"},{"content":"\n1 Procedure of EDTA\nA typical chemical reaction of a slag could be like the following [NIST, D.P Bentz],\nC7.88S7.39M3A + 2.6CH + bH → 7.39C1.42SHmA0.046 + 0.66M4.6AHd\nC=CaO, S=SiO2, M=MgO, A=Al2 O3, CH=Ca(OH)2, H=H2O.\nThe method EDTA (Ethylenediaminetetraacetic acid) has been described by Erntroy [Erntry, 1987]. The following is a short description of the method.\n93.0g of disodium EDTA 2H2O is dissolved in a mixture of 250 ml triethanolamine and 500 ml water. The solution is transferred to an volumetric flask; 173 ml of diethylamine added and the mixture made up to 1000 ml with water; For the extraction, 50 ml of the above solution is pipetted into a beaker and diluted to approximately 800 ml with water; The solution is brought to a temperature of 20.0±2 ◦C and 0.5 g of the dried and powdered sample paste, weighed to the nearest 0.0001 g, sprinkled over its surface; The solution is stirred for 120 ± 5 min while maintaining the stated temperature and is then filtered under vacuum through a 90 mm diameter Whatman GF/C filter which had been previously washed with 100 ml of distilled water, dried and weighed; The residue is then washed 5 times with 10 ml lots of distilled water, fried at 105 ◦ C for 1 hour and weighed to the nearest 0.0001 g. Calculation of reaction degree of slag. 2 Calculation of reaction degree of slag\nTake Msl g slag and MCH g Ca(OH)2 and MH g H2O as reactant. When the test age reaches, say 3 days, take two pieces of paste, dry and weigh them, then,\none is ground to powder for EDTA test; the other piece undergoes a ignition loss test (LOI), from the LOI, the slag mass fraction in the dried paste powder can be determined, the ignition loss of CH should be taken into account, for Ca(OH)2 is decomposed to CaO and H2O. The LOI fraction is: fLOI, thus, 1 − fLOI is the mass fraction of CaO+slag, so the original slag content in the powder can be determined.\n2.1 Correction of hydrotalcite\nh= Mass of dried hydrotalcite formed from 1 g of MgO in the slag glass.\nThe value of h could be 2.35 g based on the assumption in the paper \u0026ldquo;Degrees of reaction of the slag in some blends with Portland cement\u0026rdquo;, there the hydrotalcite is considered as M5ACH7.\nTherefore, the residue of slag should minus the residue formed from MgO. The content of MgO can be determined by the content of slag of the tested powder.\n2.2 Correction of slag\nA small amount of slag may be solved in the reagent EDTA solution.\nIt is better do a pure unreacted slag test using EDTA, to determine the fraction of slag dissolution.\nIf the dissolution of slag in EDTA is quite small, then there is no need to take account for correction for solved unreacted slag in EDTA reagent, assuming no unreacted slag is solved in the EDTA solution.\nA well formatted file (PDF) of the content on this webpage may be downloaded via this link.\n","permalink":"https://www.cementscience.com/2012/12/determining-the-amount-of-reacted-slag-in-blended-cement-using-edta-method.html","summary":"\u003cp\u003e\u003cimg alt=\"EDTA-slag\" loading=\"lazy\" src=\"/wp-content/uploads/2012/12/EDTA-slag.jpg\"\u003e\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003e1 Procedure of EDTA\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eA typical chemical reaction of a slag could be like the following [NIST, D.P Bentz],\u003c/p\u003e\n\u003cp\u003eC7.88S7.39M3A + 2.6CH + bH → 7.39C1.42SHmA0.046 + 0.66M4.6AHd\u003c/p\u003e\n\u003cp\u003eC=CaO, S=SiO2, M=MgO, A=Al2 O3, CH=Ca(OH)2, H=H2O.\u003c/p\u003e\n\u003cp\u003eThe method \u003ca href=\"https://www.cementscience.com/2012/07/methods-to-measure-the-reaction-degree-of-slag-in-blended-cement.html\"\u003eEDTA\u003c/a\u003e (Ethylenediaminetetraacetic acid) has been described by Erntroy [Erntry, 1987]. The following is a short description of the method.\u003c/p\u003e\n\u003cul\u003e\n\u003cli\u003e\n\u003col\u003e\n\u003cli\u003e93.0g of disodium EDTA 2H2O is dissolved in a mixture of 250 ml triethanolamine and 500 ml water. The solution is transferred to an volumetric flask;\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"2\"\u003e\n\u003cli\u003e173 ml of diethylamine added and the mixture made up to 1000 ml with water;\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"3\"\u003e\n\u003cli\u003eFor the extraction, 50 ml of the above solution is pipetted into a beaker and diluted to approximately 800 ml with water;\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"4\"\u003e\n\u003cli\u003eThe solution is brought to a temperature of 20.0±2 ◦C and 0.5 g of the dried and powdered sample paste, weighed to the nearest 0.0001 g, sprinkled over its surface;\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"5\"\u003e\n\u003cli\u003eThe solution is stirred for 120 ± 5 min while maintaining the stated temperature and is then filtered under vacuum through a 90 mm diameter Whatman GF/C filter which had been previously washed with 100 ml of distilled water, dried and weighed;\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"6\"\u003e\n\u003cli\u003eThe residue is then washed 5 times with 10 ml lots of distilled water, fried at 105 ◦ C for 1 hour and weighed to the nearest 0.0001 g.\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003cli\u003e\n\u003col start=\"7\"\u003e\n\u003cli\u003eCalculation of reaction degree of slag.\u003c/li\u003e\n\u003c/ol\u003e\n\u003c/li\u003e\n\u003c/ul\u003e\n\u003cp\u003e\u003cstrong\u003e2 Calculation of reaction degree of slag\u003c/strong\u003e\u003c/p\u003e","title":"Determining the Amount of Reacted Slag in Blended Cement Using EDTA Method"},{"content":"When we simulate the hydration process of Portland cement, it is of significant importance to know the hydration mechanisms. Basically, there are two mechanisms for the hydration of Portland cement, viz. Topochemical and Through-Solution Reaction.\n1 Topochemical Reaction Concept\nImmediately after the first contact of the cement with water a calcium-rich silicious clinker would liberate Ca2+ ions into the solution. A calcium-poor skeleton is left which reacts with the calcium-rich solution which is accompanied by swelling of the hydration products compared with the original volume of the anhydrous cement.\nThe topochemical concept was launched by Michaelis at the beginning of last century. Since then topochemical phenomena have been reported for the hydration of both C3S and Portland cement.\nSchematic representation of proposed hydration mechanisms\n2 Through-Solution Concept\nIn the through-solution concept dissolution of the anhydrous grain after contact of the cement with water is considered to be followed by hydration in the solution. The hydration products then precipitate on the grain surface.\nThe through-solution concept was first formulated by Le Chatelier for plaster and Portland cement in the first decade of this century. The concept has been supported by many reserachers, Regourd et al., Brunauer and Gauglitz, Williamson and Dron et al.\nThe debate on whether cement hydration proceeds topochemically or according to a through-solution mechanism dates back to the very beginning of cement chemistry. The subject is of significant importance in view of mathematical modeling of both the hydration process and structural formation. As such, a so-called Simultaneously Operating Mechanisms is proposed to account for the debate.\n3 Simultaneously Operating Mechanisms\nAccording to Neville the controversy between the topochemical and through-solution concept can largely be reduced to a matter of terminology. Shebl et al. explains that hydration of C3S involves both through-solution reactions and topochemical reactions (solid-state reaction). The water/solid ratio would be an important factor in this respect. For low water/solid ratios the reaction would be predominantly topochemical, whereas for high water/solid ratios the through-solution mechanism would be more important. Both reactions could occur simultaneously.\nThe concept of simultaneously operating mechanisms is plausible indeed if the outer products, i.e. the products which are formed outside the original grain boundaries in a relatively water-rich environment, are formed by a through-solution mechanism, while the inner products, formed inside the original grain boundaries, are the result of a topochemical reaction.\nFrom a literature survey on this topic Daimon concluded that it is very difficult to determine which mechanism has marred. The fact that we are dealing with a poly-size system significantly contributes to the complexity of the subject. Probably the effect of the particle size distribution also explains why Kalousek found many contradictions between different authors on this point.\nThe conclusion is that the mechanism of cement hydration depends on the water/solid ratio, viz. low water/solid ratios lead to topochemical reaction, while through-solution mechanism is more important at high water/solid ratios, and both reactions could occur simultaneously.\nReference: Simulation of hydration and formation of structure in hardening cement-based materials, by K. Van Breugel, TuDelft.\n","permalink":"https://www.cementscience.com/2012/11/hydration-mechanisms-of-portland-cement-topochemical-or-through-solution-reaction.html","summary":"\u003cp\u003eWhen we \u003ca href=\"https://www.cementscience.com/2012/05/two-main-methods-to-model-cement-based-materials.html\"\u003esimulate the hydration process\u003c/a\u003e of Portland cement, it is of significant importance to know the hydration mechanisms. Basically, there are two mechanisms for the hydration of Portland cement, viz. Topochemical and Through-Solution Reaction.\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003e1 Topochemical Reaction Concept\u003c/strong\u003e\u003c/p\u003e\n\u003cblockquote\u003e\n\u003cp\u003eImmediately after the first contact of the cement with water a calcium-rich silicious clinker would liberate Ca2+ ions into the solution. A calcium-poor skeleton is left which reacts with the calcium-rich solution which is accompanied by swelling of the hydration products compared with the original volume of the anhydrous cement.\u003c/p\u003e\n\u003cp\u003eThe topochemical concept was launched by Michaelis at the beginning of last century. Since then topochemical phenomena have been reported for the hydration of both C3S and Portland cement.\u003c/p\u003e\n\u003c/blockquote\u003e","title":"Hydration Mechanisms of Portland Cement: Topochemical or Through-Solution Reaction?"},{"content":"Construction industry, the only industry still does things manually.\nEven in the 21st century, to build a house right now is still a slow, labour-intensive, dangerous process, and almost always over-budget. Unlike the motoring or technology industries which use automated production methods to complete routine construction tasks, housing construction is one of the only industry that still does things manually till now, as said by Professor Khoshnevis from USC.\nIt is time to change. With the achievement of the research in 3D printing filed, Professor Khoshnevis scaled up 3D printing to make this technology being able to construct buildings by using a process called Contour Crafting. He hope to use this method to improve the basic concept of house construction so that it was accessible to everyone, because with better shelter comes a more civilized society.\nHow does 3D printer work to print a house?\nHere is how 3D printing works to \u0026ldquo;print\u0026rdquo; a house:\nA CAD design is sent to a large-scale 3D printer that is mounted to a block of land. The printer lays out the concrete-like foundation of the home through a nozzle that can move anywhere on the property. Like any 3D print-out, the house is made layer-by-layer and reinforced with various materials — like electrical, plumbing and communication infrastructure — as the build progresses.\nThe process is super fast. In a TED presentation, Prof. Khoshnevis said that “we anticipate that an average house, like 2500 square foot house, can be built in about 20 hours from a custom design”.\nAs for the material used as the \u0026ldquo;printer ink\u0026rdquo;, concrete is the solution. The concrete used in the 3D house printer is a mixture of concrete and fibre polymers, meaning that it is more than three times stronger than traditional concrete used in today’s houses. The traditional concrete can withstand roughly 3000 pounds per square inch of pressure, while the new printed concrete can withstand around 10,000 pounds per square inch.\nIs it the future of cementitious materials in construction industry?\nProfessor Khoshnevis says the method could be used to construct emergency or low-income housing. What is more, the concept is currently being supported by NASA so that the space agency can one day be used to build a colony on the Moon, and perhaps on the Mars, who knows.\nAs a cement researcher, I think the method is really revolutional in the construction industry, even just consider it from the theoretical concept. If the method is quite popular in the future, does it mean cementitious materials are the future of construction materials compared with steel? since the mixture \u0026ldquo;concrete\u0026rdquo; is the main material in the 3D printing machine used as \u0026ldquo;printing ink\u0026rdquo;.\n","permalink":"https://www.cementscience.com/2012/10/3d-printer-to-print-a-house-is-it-the-future-of-cementitious-materials.html","summary":"\u003cp\u003e\u003cstrong\u003eConstruction industry, the only industry still does things manually.\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eEven in the 21st century, to build a house right now is still a slow, labour-intensive, dangerous process, and almost always over-budget. Unlike the motoring or technology industries which use automated production methods to complete routine construction tasks, housing construction is one of the only industry that still does things manually till now, as said by Professor Khoshnevis from USC.\u003c/p\u003e\n\u003cp\u003eIt is time to change. With the achievement of the research in 3D printing filed, Professor Khoshnevis scaled up 3D printing to make this technology being able to construct buildings by using a process called Contour Crafting. He hope to use this method to improve the basic concept of house construction so that it was accessible to everyone, because with better shelter comes a more civilized society.\u003c/p\u003e","title":"3D printer to print a house, is it the future of cementitious materials?"},{"content":"How is GGBS used?\nGGBS (Ground Granulated Blastfurnace Slag) is used all over the world as a direct replacement for Portland cement. It is added to the concrete mixer along with ordinary cement, aggregates and water.\nThe normal ratios and proportions of aggregates and water to cementitious material in the mix remain unchanged. Mixing times are the same as for ordinary cement. Both wet mixing and dry mixing processes can be used for making concrete with GGBS.\nWhat is the substitution rates of GGBS in concrete?\nUsually, replacement rates for GGBS vary from 30% to up to 85%, depending on the application and technical requirements. Typically 50% is used in most instances. Higher replacement rates up to 85% are used in specialist applications such as in aggressive environments and to reduce heat of hydration.\nAccording to the EU code \u0026ldquo;EN-197-1-2000 Cement. Composition, specifications and conformity criteria for common cements\u0026rdquo;, slag in Blastfurnace cement CEM III/C can be used at a substitution rate as high as 95%.\nBelow are some typical Substitution Rates\nReady-mix Concrete: 50% GGBS is used for most mixes.\nPrecast Concrete: 30% to 50% GGBS primarily depending on concrete curing conditions.\nSpecial Concrete: Mass concrete typically has at least 70% GGBS for temperature control. Concrete in aggressive environments usually contains from 50% to 70% GGBS for enhanced durability performance.\n","permalink":"https://www.cementscience.com/2012/10/how-ggbs-is-used-and-its-typical-substitution-rates.html","summary":"\u003cp\u003e\u003cstrong\u003eHow is GGBS used?\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eGGBS (Ground Granulated Blastfurnace Slag) is used all over the world as a direct replacement for Portland cement. It is added to the concrete mixer along with ordinary cement, aggregates and water.\u003c/p\u003e\n\u003cp\u003eThe normal ratios and proportions of aggregates and water to cementitious material in the mix remain unchanged. Mixing times are the same as for ordinary cement. Both wet mixing and dry mixing processes can be used for making concrete with GGBS.\u003c/p\u003e","title":"How GGBS is used and its typical substitution rates"},{"content":"Among the conferences taking place every year on cement science, International Congress of Cement Chemistry (ICCC) is almost the most important one. The conference takes place every four years. The latest one is the 13th ICCC hosted in Madrid Spain in 2011 and the next one 14th ICCC will be hosted in Beijing in 2015. During the 13th ICCC, there were more than 900 participants from over 60 countries all over the world, received more than 400 papers on cement science, which cover 9 subjects:\n1.- Production process chemistry and engineering 2.- Sustainable production 3.- New cementitious matrix 4.- Hydration and microstructure 5.- Hydration and thermodynamics 6.- Modelling 7.- Properties of fresh and hardened concrete 8.- Concrete durability 9.- Standardization When reading papers, I saw numerous researchers refer to the information from the papers of ICCC, unfortunately, those proceedings of earlier age are not easy to find, since they are no digital version (like PDF files), or they are not open to the public. Even for the latest proceedings, you have to attend the meetings to get the proceedings, but the cost to attend these meetings is expensive or at least not cheap. What is even worse is that every meeting is definitely not available for all people in the field, due to the difficulties such as travelling and time schedule.\nThe purpose of conference is to gather people who are interested on some issues in the same field to discuss and share latest results. As a result of meetings, the proceedings paper is a good media to store and spread these information. So we should make these proceedings open for the related researchers rather than close them for a small group of researchers, which is not the REAL Science, Science should be OPEN, and must be OPEN.\nI have attended the 13th ICCC thanks to the financial support from my promoter, and got a digital proceedings of the conference. I think it is a good idea to share them with you who are also a researcher on cement science. Just click the link Proceedings of 13th International Congress on the Chemistry of Cement to download them onto your computer or copy the whole folder to your DropBox account.\nShare them and make science OPEN.\n","permalink":"https://www.cementscience.com/2012/10/proceedings-of-13th-international-congress-on-the-chemistry-of-cement.html","summary":"\u003cp\u003eAmong the conferences taking place every year on cement science, International Congress of Cement Chemistry (ICCC) is almost the most important one. The conference takes place every four years. The latest one is the 13th ICCC hosted in Madrid Spain in 2011 and the next one 14th ICCC will be hosted in Beijing in 2015. During the 13th ICCC, there were more than 900 participants from over 60 countries all over the world, received more than 400 papers on cement science, which cover 9 subjects:\u003c/p\u003e","title":"Proceedings of 13th International Congress on the Chemistry of Cement"},{"content":"Better performance of slag concrete exposing to high temperatures\nConcrete made with GGBS cement is much better than concrete made with 100% OPC at maintaining its compressive strength when exposed to high temperatures.\nOPC specimens heated to 400 °C or above have been shown to exhibit severe cracking to the point of disintegration after a few days. However, it was found that concrete made with blends of 35%, 50% and 65% GGBS performed much better. In the GGBS specimens there was no visible cracking after exposure to the higher temperatures. The concrete with 100% OPC degraded to powder over the following year, while the concrete made with GGBS maintained its strength over the same period.\nFurther studies showed that after exposure to 900 °C concrete with 0% GGBS maintained 6% of its original strength, concrete with 30% GGBS maintained 54% of its original strength and concrete with 70% GGBS maintained 70% of its original strength.\nDate source: Ecocem.\nHow does slag improve the resistance to fire damage?\nWhy concrete made with GGBS has better resistance to fire damage? It is generally agreed that above 400 °C Ca(OH)2 which is the hydration products of OPC decomposes into CaO and H2O, then on cooling CaO and left H2O rehydrates into Ca(OH)2 which needs more space than CaO causing the concrete to crack and degrade. With the addition of GGBS into concrete, hydration product Ca(OH)2 is generally reduced compared with concrete made with 100% OPC, thus improving the performance of resisting fire damage.\nReference: Ecocem report\u0026ndash;Technical Performance\n","permalink":"https://www.cementscience.com/2012/10/concrete-made-with-slag-improves-resistance-to-fire-damage.html","summary":"\u003cp\u003e\u003cstrong\u003eBetter performance of slag concrete exposing to high temperatures\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eConcrete made with \u003ca href=\"https://www.cementscience.com/2012/05/introduction-slag-cement.html\"\u003eGGBS cement\u003c/a\u003e is much better than concrete made with 100% OPC at maintaining its compressive strength when exposed to high temperatures.\u003c/p\u003e\n\u003cp\u003eOPC specimens heated to 400 °C or above have been shown to exhibit severe cracking to the point of disintegration after a few days. However, it was found that concrete made with blends of 35%, 50% and 65% GGBS performed much better. In the GGBS specimens there was no visible cracking after exposure to the higher temperatures. The concrete with 100% OPC degraded to powder over the following year, while the concrete made with GGBS maintained its strength over the same period.\u003c/p\u003e","title":"Concrete made with slag improves resistance to fire damage"},{"content":"As a cement researcher, I know cement much better than average people, while it is not the case with everything with a name using the word \u0026ldquo;cement\u0026rdquo;.\nWhen I type \u0026ldquo;cement\u0026rdquo; in the powerful Google search box, Google automatically gives an alternative search phrase \u0026ldquo;cement mixer shot\u0026rdquo;, which means \u0026ldquo;cement mixer shot\u0026rdquo; is a very popular searchable phrase on the Internet.\nI know concrete mixer, and even cement mixer, for they are machines used to mix concrete and cement, but what is \u0026ldquo;cement mixer shot\u0026rdquo;?\nFollowing the information suggested by Google, cement mixer shot is a kind of shot drink, usually consists of:\n1 part Bailey\u0026rsquo;s Irish Cream (Other types of alcoholic Irish cream may be substituted.) 1 part Lime juice (lemon juice may be substituted)\nHow to make a Cement Mixer Shot? below are two recipes for making Cement Mixer Shot:\nCement Kicker recipe\n1 shot Bailey\u0026rsquo;s Irish cream 1/2 shot lime juice 1/2 shot 151 proof rum\nFill one shot glass with Bailey\u0026rsquo;s. Fill second shot glass with Lime and 151.\nTo Drink: Pour Bailey\u0026rsquo;s into mouth, do not swallow. Pour Lime and 151 into mouth. Shake head back and fourth, the shot will turn solid.\nServe in: Shot Glass\nCement Mixer recipe\n1 jigger Bailey\u0026rsquo;s Irish cream 1 jigger lime juice\nHold one shot of bailey\u0026rsquo;s in your mouth, and take one shot of lime juice. Mix rapidly in mouth by shaking head vigorously, then consume.\nAs showed by About.com, an interesting chemical reaction takes place in a shot glass when a Cement Mixer is made. As the shot sits, the Bailey’s and lime juice slowly mix together creating a thick slurry best compared to cottage cheese.\nActually, cement mixer is a cocktail that has seen increasing popularity among older college students, in an effort to prevent or discourage underage drinking, by serving or offering it to a student who may be lying about his or her age, as when not prepared the right way, the curdling of the milk in the drink can cause an upset stomach, diarrhea, nausea, and/or vomiting.\nAn important trick when drinking a Cement Mixer is timing: don’t wait too long otherwise the mix will become too thick. Beyond this, cement mixer is not a good tasting mix, consider it more of a gag shot when playing this trick on someone.\nThe world is too colorful to be explored, even as a so-called cement expert, I did not know a drink named \u0026ldquo;cement mixer\u0026rdquo; lies out there. Is it funny?\n","permalink":"https://www.cementscience.com/2012/09/what-is-cement-mixer-shot.html","summary":"\u003cp\u003eAs a cement researcher, I know \u003ca href=\"https://www.cementscience.com/2012/07/what-is-cement-and-its-history.html\"\u003e\u003cstrong\u003ecement\u003c/strong\u003e\u003c/a\u003e much better than average people, while it is not the case with everything with a name using the word \u0026ldquo;cement\u0026rdquo;.\u003c/p\u003e\n\u003cp\u003eWhen I type \u0026ldquo;cement\u0026rdquo; in the powerful Google search box, Google automatically gives an alternative search phrase \u0026ldquo;cement mixer shot\u0026rdquo;, which means \u0026ldquo;cement mixer shot\u0026rdquo; is a very popular searchable phrase on the Internet.\u003c/p\u003e\n\u003cp\u003eI know concrete mixer, and even cement mixer, for they are machines used to mix concrete and cement, but what is \u0026ldquo;cement mixer shot\u0026rdquo;?\u003c/p\u003e","title":"What is Cement Mixer Shot?"},{"content":"In the cement science field, XRD analysis combined with Rietveld method can give quantitative results of crystalline phase of hydration products, so I try to use XRD/Rietveld method to quantify the hydration products of cementitous material. To achieve good performance of XRD test, fine powder is required and of great importance.\nThe question is how fine the particle sizes should be? It is showed by research that the particle size of powder has to be reduced to 10 μm or less, which is especially important for quantitative analysis (Smith, 2001).\nHere comes the problem, it is very difficult to obtain these grain sizes by hand grinding, which means that mechanical grinding is required to reduce the grain size sufficiently.\nThere are several points should be stated. For soft minerals such as zeolites (hardness 3–4) grinding can introduce problems of size broadening and amorphous layers can be formed around grains. Prolonged grinding can even make the minerals completely X-ray amorphous (Okada et al., 1993; Kosanovic et al., 1993). Wet grinding generally lowers these effects, but in ball mills even wet grinding can still lead to problems of amorphization and line broadening (Okada et al, 1993).\nBy the help of Dr. Lieven MACHIELS from KuLeuven, it is reported in his doctor thesis that several authors have shown that wet grinding using a McCrone Micronizing mill is the most efficient method of reducing the particle size of most materials, while avoiding many of the deleterious effects that can be associated with mechanical grinding (O’Connor and Chang, 1986; Buhrke et al., 1998; Eberl, 2003).\nTherefore, we applied the method to grind hydrated pastes to get particles smaller than 10 μm for XRD analysis. In the future, we will analyze and assess whether this method is good enough to obtain quantitative results.\n","permalink":"https://www.cementscience.com/2012/09/sample-preparation-by-mccrone-micronizing-mill-before-xrdrietveld-test.html","summary":"\u003cp\u003eIn the cement science field, XRD analysis combined with Rietveld method can give quantitative results of crystalline phase of hydration products, so I try to use XRD/Rietveld method to quantify the hydration products of cementitous material. To achieve good performance of \u003ca href=\"https://www.cementscience.com/2012/06/hydration-products-of-slag-in-blended-cement.html\"\u003eXRD\u003c/a\u003e test, fine powder is required and of great importance.\u003c/p\u003e\n\u003cp\u003eThe question is how fine the particle sizes should be? It is showed by research that the particle size of powder has to be reduced to 10 μm or less, which is especially important for quantitative analysis (Smith, 2001).\u003c/p\u003e","title":"Sample preparation by McCrone Micronizing mill before XRD/Rietveld test"},{"content":"Twitter | Facebook\nHow to contact me?\nThe best way to contact me is Email: Zhijun.Tan#TanZhijun.com (please use @ instead of #, I hate spams). Other tools such as MSN and Skype are not my favorites, so I would not give you them here.\nShould you have any question or would like to contact with me, feel free to email me, you are warmly welcome.\nI guess some friends hate boring email. Facing the overwhelming social media, you can also follow me at Twitter, Facebook or Google+ by clicking the following links.\nLinkedIn Twitter Facebook\n","permalink":"https://www.cementscience.com/contact/","summary":"\u003cp\u003e\u003ca href=\"https://twitter.com/tumutanzi\"\u003eTwitter\u003c/a\u003e | \u003ca href=\"https://www.facebook.com/tumutanzi\"\u003eFacebook\u003c/a\u003e\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003eHow to contact me?\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eThe best way to contact me is Email: Zhijun.Tan#TanZhijun.com (please use @ instead of #, I hate spams). Other tools such as MSN and Skype are not my favorites, so I would not give you them here.\u003c/p\u003e\n\u003cp\u003eShould you have any question or would like to contact with me, feel free to email me, you are warmly welcome.\u003c/p\u003e\n\u003cp\u003eI guess some friends hate boring email. Facing the overwhelming social media, you can also follow me at Twitter, Facebook or Google+ by clicking the following links.\u003c/p\u003e","title":"Contact"},{"content":"Some other websites on cement or concrete materials are listed below.\nCements@Sheffield Microlab-m3c4.blogspot.com Csla-project.blogspot.com www.nationalslag.org www.slagcement.org www.cembureau.eu www.globalslag.com www.globalcement.com ","permalink":"https://www.cementscience.com/links/","summary":"\u003cp\u003eSome other websites on cement or concrete materials are listed below.\u003c/p\u003e\n\u003cul\u003e\n\u003cli\u003e\u003ca href=\"http://cements.group.shef.ac.uk/\"\u003eCements@Sheffield\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://microlab-m3c4.blogspot.com/\"\u003eMicrolab-m3c4.blogspot.com\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.csla-project.blogspot.com/\"\u003eCsla-project.blogspot.com\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.nationalslag.org/\"\u003ewww.nationalslag.org\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.slagcement.org/\"\u003ewww.slagcement.org\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.cembureau.eu\"\u003ewww.cembureau.eu\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.globalslag.com/\"\u003ewww.globalslag.com\u003c/a\u003e\u003c/li\u003e\n\u003cli\u003e\u003ca href=\"http://www.globalcement.com/\"\u003ewww.globalcement.com\u003c/a\u003e\u003c/li\u003e\n\u003c/ul\u003e","title":"Links"},{"content":"It is mentioned previously that the reactivity of slag is influenced by its fineness of grinding (specific surface area) that is determined by the sizes of slag particles. The finer the slag particles, the larger the surface area, which means higher hydration degree of slag.\nHowever, if disregarding the fineness, in other words, take two slag particles with significantly different sizes (diameters of \u0026ldquo;spherical\u0026rdquo; particles) as the study target, do the reacting front layers of the two particles grow at same rate? The growing rate of reacting layer can be a good tool to calculate the hydration degree of slag at particle level.\nSimulated results conducted by Wei Chen showed the thickness of the hydrated layer is not significantly influenced by the particles size of slags, which is in good agreement with experiment result in which Na(OH)2 solution was used as activator [Ref. Three-dimensional computer modeling of slag cement hydration].\nAnother research carried out in 1986 reported similar result: \u0026ldquo;the thickness of hydrated layer of particle did not depend on the particle size, that is, the hydration reactivity had nothing to do with particle size and the rate of hydration was actually in proportion to the total surface area.\u0026rdquo; Detailed information is quoted as follows [Ref. Hydration of blast furnace slag particle, from 8th International Congress on the Chemistry of Cement Vol 4 (1986) Pages: 98-103],\nIt is most practical to evaluate the hydraulic reactivity of water granulated blast furnace slag in terras of the strength of hardened body. In order to make the extensive use of slag, however, it is important to investigate the hydration properties of individual particles. Hydration properties mainly investigated here were the change in the amount of hydration and the thickness of hydrated layer with time, and the effect of alkaline activator.\nWe examined the hydration of ground commercial slag with various particle sizes. Experiment was carried out as follows: samples with five different particle sizes (3.27, 4.05, 5.86, 8.66 and 13.36 μm by volume mean diameter) were prepared. They were hydrated in suspension with the water-slag ratio of 10 with NaOH, Ca(OH)2 or ordinary Portland cement as alkaline activator.\nThe amount of hydration of the slag under such an alkali-condition was measured by determining the soluble part of the hydration product using salicylic acid-acetone-methanol solution, and also by loss on ignition.\nThe following results were obtained. The thickness of hydrated layer of particle did not depend on the particle size, that is, the hydration reactivity had nothing to do with particle size and the rate of hydration was actually in proportion to the total surface area. It was suggested, on the other hand, that each alkaline activator show the characteristic effect on the hydration of each sample. Some of these results were supported by further experiments.\nAccording to these research results, it is concluded that the reactivity of slag has nothing to do with particle size at particle level, while the surface area (fineness) determines hydration degree of slag.\nIt is should be noted that the two research results mentioned here only cover a narrow particle size distribution (0-15 micrometers). To apply this conclusion to wide size range, further research work is needed.\n","permalink":"https://www.cementscience.com/2012/09/does-particle-size-of-slag-influence-its-reactivity.html","summary":"\u003cp\u003eIt is mentioned previously that the reactivity of slag is \u003ca href=\"https://www.cementscience.com/2012/07/factors-influence-the-reaction-degree-of-slag-in-slag-blended-cement.html\"\u003einfluenced by its fineness of grinding\u003c/a\u003e (specific surface area) that is determined by the sizes of slag particles. The finer the slag particles, the larger the surface area, which means higher hydration degree of slag.\u003c/p\u003e\n\u003cp\u003eHowever, if disregarding the fineness, in other words, take two slag particles with significantly different sizes (diameters of \u0026ldquo;spherical\u0026rdquo; particles) as the study target, do the reacting front layers of the two particles grow at same rate? The growing rate of reacting layer can be a good tool to calculate the hydration degree of slag at particle level.\u003c/p\u003e","title":"Does particle size of slag influence its reactivity?"},{"content":"Granulated Blast Furnace Slag (GGBFS, or GGBFS, or BFS) is the most used material in cement industry to make slag cement. How is GBFS made? What are the processing and its applications?\nProcess: water quenching\nGenerally speaking, GBFS is formed by water quenching. The glassy and granular material is generated when slag is rapidly chilled by immersion in water.\nThe most common process for granulating blast furnace slag involves the use of high water volume, high pressure water jets in direct contact with the molten blast furnace slag at a ratio of approximately 10 to 1 by mass. The molten blast furnace slag is quenched almost immediately to form a material generally smaller than a #4 sieve.\nThe efficiency, which the molten blast furnace slag is rapidly chilled, as well as the chemical composition of the slag source, largely determines its cementitious properties for use in concrete. After the granulated blast furnace slag is formed, it must be dewatered, dried and ground, using processes similar to those used with Portland cement clinker to make Portland cement.\nTypically, granulated slag is ground to an air-permeability (blaine) fineness exceeding that of Portland cement to obtain increased hydraulic activity at early ages. As with Portland cement and pozzolans, the rate of reaction increases with the particle fineness.\nGround Granulated Blast Furnace Slag (GGBFS) is activated by alkalis or Ca(OH)2 etc.\nGBFS has to be grind to get Ground Granulated Blast Furnace Slag (GGBFS) having large fineness.When GGBFS is mixed with water, initial hydration is much slower as compared with Portland cement. Therefore, Portland cement or alkali salts are used to increase the reaction rate. In the hydration process, GGBFS produces calcium silicate hydrate cement paste. This valuable contribution fromGGBFS improves the paste-to-aggregate bond in concrete. GGBFS mixtures with Portland cement typically result in greater strength and reduced permeability.\nColor of GGBFS\nGGBFS is considerably lighter in color than most Portland cements and will produce a lighter concrete end product. Occasionally, concrete containing GGBFS may exhibit a blue-green coloration. While this coloration effect seldom occurs, it is attributed to a complex reaction of the sulfide sulfur in the GGBFS with other compounds in the cement and will diminish with age.\nGeneral applications of GGBFS\nraw material for the manufacture of cement lightweight fill raw material for the manufacture of glass Factors affecting cementitious properties of GGBFS\nchemical composition of GGBFS alkali concentration of the reacting system glass content of the GGBFS fineness of the GGBFS and Portland cement. Added value of GBFS using in concrete applications\nreduced chloride permeability improved resistance to sulfate attack reduced heat of hydration in mass concrete improved compressive and flexural strength reduced alkali-silica reaction Reference: http://www.nationalslag.org/\n","permalink":"https://www.cementscience.com/2012/09/processing-of-granulated-blast-furnace-slag-and-its-applications.html","summary":"\u003cp\u003eGranulated Blast Furnace Slag (GGBFS, or GGBFS, or BFS) is the most used material in cement industry to make slag cement. How is GBFS made? What are the processing and its applications?\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003eProcess: water quenching\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eGenerally speaking, GBFS is formed by water quenching. The glassy and granular material is generated when slag is rapidly chilled by immersion in water.\u003c/p\u003e\n\u003cp\u003eThe most common process for granulating blast furnace slag involves the use of high water volume, high pressure water jets in direct contact with the molten blast furnace slag at a ratio of approximately 10 to 1 by mass. The molten blast furnace slag is quenched almost immediately to form a material generally smaller than a #4 sieve.\u003c/p\u003e","title":"Processing of Granulated Blast Furnace Slag and its applications"},{"content":"Although it is somewhat difficult to measure the reaction degree of slag in slag blended cement comparing with the case in Portland cement, many researchers performed experiments on this field. A large body of literature can be found on the kinetics of Portland cement/slag blends.\nBased on the modification of Takashima’s salicylic acid extraction method, Taylor collected some researchers\u0026rsquo; data on the reaction degree of slag, as is showed in Table 1.\nTable 1. Data on reaction degree of slag in blended cement from literature.\nOther researchers using EDTA or DTA also reported data on this issue under different hydration conditions; Table 2 is an uncompleted collection of these data.\nTable 2. Uncompleted data collection of reaction degree of slag blended cement.\nBy means of EDTA extraction method, the work of Lumley et al. focused on the effect of water to solid ratios and the proportions of slag on the degrees of reaction of slag blending with Portland cement. It is reported that at water to solids ratios of 0.4-0.6 and 20 °C 30-55% of the slag reacts in 28 days and 45-75% in 1-2 years, for blends containing 92% slag and w/s=0.3, the hydration degree of slag is probably limited to 30%.\nThey also found that at water/solid ratio 0.3 the composition of Portland cement, even with an inclusion of 5% gypsum, has no significant effect on the degrees of slag reaction in the blend at ages of 28 days to 1 year.\nLuke and Glasser reported that approximate 40% of the slag in a 30%/70% ratio of slag to Portland cement blend reacted in one month with little change up to 6 months, but over 60% of slag was reacted at the age of 12 months. Their latter study showed similar results with data at 25 °C, 40 °C and 50 °C for times of 0.5 to 24 months.\n","permalink":"https://www.cementscience.com/2012/08/published-literature-data-on-the-reaction-degree-of-slag.html","summary":"\u003cp\u003eAlthough it is somewhat difficult to measure the \u003ca href=\"https://www.cementscience.com/2012/07/kinetics-of-cement-degree-of-hydration-or-degree-of-reaction.html\"\u003ereaction degree\u003c/a\u003e of slag in slag blended cement comparing with the case in Portland cement, many researchers performed experiments on this field. A large body of literature can be found on the kinetics of Portland cement/slag blends.\u003c/p\u003e\n\u003cp\u003eBased on the modification of Takashima’s salicylic acid extraction method, Taylor collected some researchers\u0026rsquo; data on the reaction degree of slag, as is showed in Table 1.\u003c/p\u003e","title":"Published literature data on the reaction degree of slag"},{"content":"It is so common to see the terms \u0026ldquo;degree of hydration\u0026rdquo; and \u0026ldquo;degree of reaction\u0026rdquo; in research field of cemetitious material, such as cement or blended cement, especially when we focus on the kinetics.\nHere comes the question, what is the difference between the two terms? are they actually the same meaning? I was confused by the two terms when I read a huge number of papers and found not so many researchers make them clear or maybe they do not realize the difference either.\nDegree of hydration, α, as a function of curing time (By Raymond A. Cook).\nFirst, let\u0026rsquo;s know what cement hydration is? it means chemical combination of cement and water. Then what is hydration degree of cement? “Degree of hydration” of cement is defined as the fraction of Portland clinker (including gypsum addition) that has fully reacted with water.\nThere is no need to explain the meaning of word \u0026ldquo;reaction\u0026rdquo;. However, “Degree of reaction” of cement is defined as the fraction of Portland clinker (including gypsum addition) that has already fully reacted with water relative to the final reacted cement.\nFrom the two definitions for the two terms, the difference is clear. Degree of hydration does not consider the fact that ultimate hydration, i.e. hydration degree is 100%, does not occur in reality. While degree of reaction is defined as the reacted part relative to the whole part that will be finally reacted, in other words, 100% reaction degree is possible.\nBecause complete hydration of cement does not happen, ultimate hydration degree of cement is introduced. For Portland cement the ultimate degree of hydration can be calculated using Mill’s formula. Reference value of ultimate hydration degree of Portland cement (water-to-cement ratio ≈ 0.5) could be 75%, yes, the corresponding reaction degree is 100%.\n","permalink":"https://www.cementscience.com/2012/07/kinetics-of-cement-degree-of-hydration-or-degree-of-reaction.html","summary":"\u003cp\u003eIt is so common to see the terms \u0026ldquo;degree of hydration\u0026rdquo; and \u0026ldquo;degree of reaction\u0026rdquo; in research field of cemetitious material, such as cement or blended cement, especially when we focus on the \u003ca href=\"https://www.cementscience.com/2012/07/factors-influence-the-reaction-degree-of-slag-in-slag-blended-cement.html\"\u003ekinetics\u003c/a\u003e.\u003c/p\u003e\n\u003cp\u003eHere comes the question, what is the difference between the two terms? are they actually the same meaning? I was confused by the two terms when I read a huge number of papers and found not so many researchers make them clear or maybe they do not realize the difference either.\u003c/p\u003e","title":"Kinetics of cement: Degree of hydration or Degree of reaction?"},{"content":"The reaction degree of slag in blended cement is difficult to measure using those methods which are successfully applied for Portland cement. Demoulian et al. described a method based on extraction of the constituents other than unreacted slag with a reagent based on Ethylene Diamine Tetraacetic Acid (EDTA), finding it effective for determining reaction degree of slag in unhydrated blended cements.\nEDTA has long been the most used and well-known method to measure the reaction degree of slag in blended cement; however, as stated by Luke and Glasser, special care should be taken when applying this method, e.g. systematic error may occur due to the residue of hydrotalcite in the extraction of unreacted slag.\nLumley et al. reported that EDTA extraction method can be used to determine the degree of reaction of slag under certain corrections, but the accuracy is poorer at degrees of reaction above 70%.\nSource: WikiPedia.com\nBesides EDTA method, SEM-BSE image analysis could be applied to directly estimate the hydration degree of both plain cement and blended cement paste. This method is based on the fact that cement and slag grains can be distinguished from unhydrated clinkers and paste matrix, though there is some overlap due to the similar gray levels of cement and slag. However, it should be bore in mind that using this method may produces an over-estimated result on the reaction degree of slag due to its fine particles (G. Ye).\nTo improve the precise of ESEM image analysis determining the reaction degree of slag, V. Kocaba studied SEM-IA-Mg-mapping method to clearly distinguish slag phase from clinkers. The methodology is based on the Mg element of slag does move during the hydration process, thus the presence of Mg can mark the unreacted slag phase. The disadvantage of this method is extremely time consuming, which is the drawback of SEM-BSE image analysis as well.\nAs a conclusion,there is no perfect method so far to determine the reaction degree of slag in blended cements. The best solution may be using more than one method to validate each other and get reliable result.\n","permalink":"https://www.cementscience.com/2012/07/methods-to-measure-the-reaction-degree-of-slag-in-blended-cement.html","summary":"\u003cp\u003eThe \u003ca href=\"https://www.cementscience.com/2012/07/factors-influence-the-reaction-degree-of-slag-in-slag-blended-cement.html\"\u003ereaction degree of slag\u003c/a\u003e in blended cement is difficult to measure using those methods which are successfully applied for Portland cement. Demoulian et al. described a method based on extraction of the constituents other than unreacted slag with a reagent based on Ethylene Diamine Tetraacetic Acid (EDTA), finding it effective for determining reaction degree of slag in unhydrated blended cements.\u003c/p\u003e\n\u003cp\u003eEDTA has long been the most used and well-known method to measure the reaction degree of slag in blended cement; however, as stated by Luke and Glasser, special care should be taken when applying this method, e.g. systematic error may occur due to the residue of hydrotalcite in the extraction of unreacted slag.\u003c/p\u003e","title":"Methods to measure the reaction degree of slag in blended cement"},{"content":"\nSeveral days ago, I posted that the global cement output is decreasing in the first half of 2012. So how about the price trend of cement worldwide? Is it increasing or not?\nInformation from different sources shows the prices of cement varies worldwide. For instance, prices of cement in South Africa had been retailing at US $186-230/ton in March of 2012. Due to an acute shortage of cement in Ghana, cement price has rapidly risen over the latest 12 months by 25% in the capital Accra and by up to 35% in rural areas.\nCompared with the expensive price in Africa, cement price in Asia except China is more or less similar to that of United States. e.g. the price in Pakistan is US $96/ton, whileit is US$101/ton in US.\nIn the biggest construction market China, cement price has been decreasing in the first two quarters of 2012, now varying at US $55/ton and still much cheaper than that in other places.\nThe price above is for Portland cement, and conversion of US dollar from local currencies is based on the rates at time of publication.\nThere is a possibility that cement price will increase soon because of increased public sector spending in the coming fiscal year that normally starts on 1 July 2012, in the meanwhile, the shrank production of cement in 2012 may account for the risen price in the coming months as well.\n","permalink":"https://www.cementscience.com/2012/07/overview-of-global-cement-price-2012.html","summary":"\u003cp\u003e\u003cimg alt=\"Overview of cement price in the world 2012\" loading=\"lazy\" src=\"/wp-content/uploads/2012/07/world-map.jpg\"\u003e\u003c/p\u003e\n\u003cp\u003eSeveral days ago, I posted that \u003ca href=\"https://www.cementscience.com/2012/07/the-worldwide-cement-output-is-decreasing-in-2012.html\"\u003ethe global cement output is decreasing\u003c/a\u003e in the first half of 2012. So how about the price trend of cement worldwide? Is it increasing or not?\u003c/p\u003e\n\u003cp\u003eInformation from \u003ca href=\"http://www.globalcement.com/magazine/latest-issue\"\u003edifferent sources\u003c/a\u003e shows the prices of cement varies worldwide. For instance, prices of cement in South Africa had been retailing at US $186-230/ton in March of 2012. Due to an acute shortage of cement in Ghana, cement price has rapidly risen over the latest 12 months by 25% in the capital Accra and by up to 35% in rural areas.\u003c/p\u003e","title":"Overview of global cement price 2012"},{"content":"The hydration kinetics of slag is generally divided into three stages: (1) a nucleation period during which product growth is accelerating, (2) a phase boundary controlled stage, and (3) a diffusion controlled stage.\nThe reaction degree of slag in blended cement is influenced by many factors. The main factors affecting the reaction of slag in blended system include the reactivity of slag that could be defined as (C+A+M)/S, the fineness of grinding (specific surface area), the vitreous fraction of slag, the replacement level of slag in blended system, the hydration temperature and the water/solids ratio.\nPrecisely, the rate of reaction of slag decreases with the decreasing water/solids ratio and with increasing proportion of slag in the blend. Higher hydration temperatures increase the reactivity of slag. However, the composition of cement and the incorporation of additional gypsum in slag blended cement have no influence on the extent of reaction of slag at ages of 28 days to 1 year, though variations in Portland cement can affect early strength. The following figure is a representation of the effect of hydration conditions and slag characteristics on the reactivity of slag.\nRepresentation of the effect of hydration conditions and slag characteristics on the reactivity of slag.\n","permalink":"https://www.cementscience.com/2012/07/factors-influence-the-reaction-degree-of-slag-in-slag-blended-cement.html","summary":"\u003cp\u003eThe hydration kinetics of slag is generally divided into three stages: (1) a nucleation period during which product growth is accelerating, (2) a phase boundary controlled stage, and (3) a diffusion controlled stage.\u003c/p\u003e\n\u003cp\u003eThe reaction degree of slag in blended cement is influenced by many factors. The main factors affecting the reaction of slag in blended system include the reactivity of slag that could be defined as (C+A+M)/S, the fineness of grinding (specific surface area), the vitreous fraction of slag, the replacement level of slag in blended system, the hydration temperature and the water/solids ratio.\u003c/p\u003e","title":"Factors influence the reaction degree of slag in slag blended cement"},{"content":"Cement, the gray and fine powder, is the most used construction material on the world. However, how many people do they know what cement is? the answer for this question from Wikipedia is as follows,\nIn the most general sense of the word, a cement is a binder, a substance that sets and hardens independently, and can bind other materials together. The word \u0026ldquo;cement\u0026rdquo; traces to the Romans, who used the term opus caementicium to describe masonry resembling modern concrete that was made from crushed rock with burnt lime as binder.\nThe reason why cement can sets and hardens independently is its hydraulic property. When cement is mixed with water, the chemical reaction occurs and produces hydration products, such as C-S-H gel, calcium hydroxide, ettringite and monosulfoaluminate. The C-S-H gel is the main material to bind different particles and resulting in the engineering strength which is needed as a construction material.Since the set and hardening process of cement is chemical reaction, so we can get cement set under water.\nCement (Source: Wikipedia)\nAs for the chemical composition of cement, there are four essential elements in cement, which are Calcium, Silicon, Aluminum and Iron. The four elements form four clinkers, namely,\nTricalcium silicate (3CaO.SiO2), (50-70%) Dicalcium silicate (2CaO.SiO2), (15-30%) Tricalcium aluminate (3CaO.Al2O3), (5-10%) Tetracalcium aluminoferrite (4CaO.Al2O3.Fe2O3), (5-15%) If you would like to know the production process how cement is made, refer to this web page or the video below.\nIt is common to see another name of cement that is Portland cement, because concrete made with cement resembled natural stone from the Isle of Portland. It worthy to note that first cement is produced by early Greeks and Romans from volcanic ash mixed with slaked lime. Unfortunately, this art was lost during the Middle Ages. The modern cement, Portland cement, is developed in England by bricklayer Joseph Aspdin in early 1800’s.\n","permalink":"https://www.cementscience.com/2012/07/what-is-cement-and-its-history.html","summary":"\u003cp\u003eCement, the gray and fine powder, is the most used construction material on the world. However, how many people do they know what cement is? the answer for this question from \u003ca href=\"http://en.wikipedia.org/wiki/Cement\"\u003eWikipedia\u003c/a\u003e is as follows,\u003c/p\u003e\n\u003cblockquote\u003e\n\u003cp\u003eIn the most general sense of the word, a cement is a binder, a substance that sets and hardens independently, and can bind other materials together. The word \u0026ldquo;cement\u0026rdquo; traces to the Romans, who used the term opus caementicium to describe masonry resembling modern concrete that was made from crushed rock with burnt lime as binder.\u003c/p\u003e\n\u003c/blockquote\u003e","title":"What is cement and its history?"},{"content":"As reported by China Daily, the official Chinese newspaper in English, China\u0026rsquo;s cement output growth drops sharply in the first five months. The output grew 5 percent from a year earlier to 793.98 million tons; however, the growth rate represented a sharp decrease of 14.3 percentage points from the same period of last year, showed by the National Development and Research Commission.\nThe reason accounting for the dropped output of cement is the economic slumps both at home and abroad, which dampened market demands. The strict regulation and control on domestic real estate by the government further reduced the demand of building materials as well. The latest news of Sany company (Sany Group loses 30% of workforce: report) also confirmed the harsh situation of construction industry in China.\nConstruction everywhere in China.\nSince China is a fast growing market of construction industry, the cement output decrease in China may also indicates the cement drop of the whole world. Because of the struggling economy worldwide and the increasing demand of less CO2 emission of cement, scientists of cement industry should spare no effort to focus on the research of cementitious materials, such as slag, fly ash and limestone blended cements, which have economic and environment benefits.\n","permalink":"https://www.cementscience.com/2012/07/the-worldwide-cement-output-is-decreasing-in-2012.html","summary":"\u003cp\u003eAs reported by China Daily, the official Chinese newspaper in English, \u003ca href=\"http://www.chinadaily.com.cn/business/2012-06/25/content_15520337.htm\"\u003eChina\u0026rsquo;s cement output growth drops sharply\u003c/a\u003e in the first five months. The output grew 5 percent from a year earlier to 793.98 million tons; however, the growth rate represented a sharp decrease of 14.3 percentage points from the same period of last year, showed by the National Development and Research Commission.\u003c/p\u003e\n\u003cp\u003eThe reason accounting for the dropped output of cement is the economic slumps both at home and abroad, which dampened market demands. The strict regulation and control on domestic real estate by the government further reduced the demand of building materials as well. The latest news of Sany company (\u003ca href=\"http://www.wantchinatimes.com/news-subclass-cnt.aspx?id=20120704000088\u0026amp;cid=1102\"\u003eSany Group loses 30% of workforce: report\u003c/a\u003e) also confirmed the harsh situation of construction industry in China.\u003c/p\u003e","title":"The worldwide cement output is decreasing in 2012"},{"content":"As it is well-known, the activation of latent slag in blended cement is implemented by calcium hydroxide (CH, Ca(OH)2) which is the main cause maintaining the high pH value of pore solution.\nThe activation happens as the break of glass layer of slag particles. However, how does the break take place in detail? Researchers have already proposed a theory to explain the process, which will be discussed in the post. The main composition of glass is SiO2, thus the break of glass layer is actually the break of chemical bond between Si and O (Si-O). In the first step, the bond Si-O is broken by hydroxyl,\nThen the other part of broken bond Si-O- further react with water (H2O), as the following reaction equation,\nBy the second step, hydroxyl is returned. The break of Si-O bond is finished. Therefore, the two steps can be combined into one equation,\nFrom the overall process, it can be seen that hydroxyl acts as activator and is not consumed.\nThis is the theory which explains the activation of slag by CH in slag blended cement.\n","permalink":"https://www.cementscience.com/2012/07/the-activation-theory-of-slag-in-blended-cement.html","summary":"\u003cp\u003eAs it is well-known, the activation of latent slag in blended cement is implemented by calcium hydroxide (CH, Ca(OH)\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e) which is the main cause maintaining the high pH value of pore solution.\u003c/p\u003e\n\u003cp\u003eThe activation happens as the break of glass layer of slag particles. However, how does the break take place in detail? Researchers have already proposed a theory to explain the process, which will be discussed in the post. The main composition of glass is SiO\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e, thus the break of glass layer is actually the break of chemical bond between Si and O (Si-O). In the first step, the bond Si-O is broken by hydroxyl,\u003c/p\u003e","title":"The activation theory of slag in blended cement"},{"content":"The morphology of inner product region derived from alite or belite is identical to those present in neat OPC paste. In mature pastes, fully hydrated small grains of both alite and GGBFS often display a coarse morphology.\nGenerally, inner product in larger grains has a dense homogeneous morphology with very fine porosity, and large slag grains often have a rim of fine textured C-S-H which can exist for many years and merge into outer product C-S-H gel. Mg, Al-rich laths or possibly platelets present within the inner product C-S-H gel, which are oriented either towards the outer boundary of the inner product or randomly even at the outer boundary.\nThe development of the plates occurs to different extents in different slag grains, possibly depending on composition and also appearing to depend on particle size considering platelets or laths typically appear very early in small grains. When the plates are very well developed they predominate over the C-S-H gel; however, in many inner product regions, even in 3 year old pastes, the plates are less well developed and a high proportion of C-S-H gel is still present. It is not obvious from observations in the early stages that the morphology in the inner product regions is plate-like, thus it is better to be described as laths or needles.\nAnother microstructural feature of the inner products is the presence of small, round and poorly crystalline particles, which are rich in iron and aluminum and also often contain significant amounts titanium.\n","permalink":"https://www.cementscience.com/2012/06/features-of-microstructure-development-in-the-inner-product-of-reacting-slag-in-blended-cement.html","summary":"\u003cp\u003eThe morphology of inner product region derived from alite or belite is identical to those present in neat OPC paste. In mature pastes, fully hydrated small grains of both alite and GGBFS often display a coarse morphology.\u003c/p\u003e\n\u003cp\u003eGenerally, inner product in larger grains has a dense homogeneous morphology with very fine porosity, and large slag grains often have a rim of fine textured C-S-H which can exist for many years and merge into outer product C-S-H gel. Mg, Al-rich laths or possibly platelets present within the inner product C-S-H gel, which are oriented either towards the outer boundary of the inner product or randomly even at the outer boundary.\u003c/p\u003e","title":"Features of microstructure development in the inner product of reacting slag in blended cement"},{"content":"Similar to Portland cement, microstructure of slag hydrate could also be classified as inner product, which formed within the boundaries of the original anhydrous grains, and outer product that formed in the originally water-filled spaces.\nThe major phases present in the outer product region of neat OPC pastes are C-S-H gel, Ca(OH)2, AFm and AFt. The addition of slag affects the morphology of the microstructure of slag blended cement. The morphology of the outer product C-S-H varies with chemical composition, viz. at high Ca/Si ratio it has a fibrillar morphology which gradually changes to foil-like with a reduction in Ca/Si ratio. In pure OPC or with low slag loading, amorphous C-S-H has a strongly linear directional characteristic being fibrillar in its appearance in the TEM. At approximate 75% GGBFS regions of foil-like C-S-H form without these linear characteristics.\nAs the slag fraction is increased, the foil-like morphology gradually replaces the fibrillar morphology. However, the fibrillar feature of C-S-H gels occurs in all blends except neat GGBFS system. Foil-like morphology may be coarser or finer, which depends on the space constraints upon the development of C-S-H gel. Although the linear and fibrillar morphology has fine porosity, its inefficient filling of space appears to leave some fairly coarse, interconnected pores, while the more evenly distributed pores of the foil-like C-S-H are probably less well interconnected, which may account for the beneficial effects of slag in reducing diffusion rates in blended pastes, thus being largely responsible for the improved durability performance.\nThe aluminate hydrates AFt and AFm can occur in all the OPC-bearing blends. These phases are found to be identical in morphology to those present in neat OPC pastes, which has a needle-like morphology. Special attention should be paid when preparing the specimen because AFt phase may suffer dehydration.\n","permalink":"https://www.cementscience.com/2012/06/features-of-microstructure-development-in-the-outer-product-of-reacting-slag-in-blended-cement.html","summary":"\u003cp\u003eSimilar to Portland cement, microstructure of slag hydrate could also be classified as inner product, which formed within the boundaries of the original anhydrous grains, and outer product that formed in the originally water-filled spaces.\u003c/p\u003e\n\u003cp\u003eThe major phases present in the outer product region of neat OPC pastes are C-S-H gel, Ca(OH)\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e, AFm and AFt. The addition of slag affects the morphology of the microstructure of slag blended cement. The morphology of the outer product C-S-H varies with chemical composition, viz. at high Ca/Si ratio it has a fibrillar morphology which gradually changes to foil-like with a reduction in Ca/Si ratio. In pure OPC or with low slag loading, amorphous C-S-H has a strongly linear directional characteristic being fibrillar in its appearance in the TEM. At approximate 75% GGBFS regions of foil-like C-S-H form without these linear characteristics.\u003c/p\u003e","title":"Features of microstructure development in the outer product of reacting slag in blended cement"},{"content":"Many XRD analysis results have shown the main hydration products of slag blended cement are essentially similar with that of pure Portland cement, except the amounts of CH found by this method or other are in varying degrees and less than those that should be given by the pure Portland cement constituent if the slag part did not participate the reaction.\nThe main hydration products of the slag-cement are C-S-H gel, Ca(OH)2, the sulpho-aluminate hydrate phases AFt and AFm and a Mg, Al-rich hydroxide phase.\nFig. 1. Transmission electron micrograph showing foil-like Op C-S-H in a water-activated slag paste hydrated for 3 1/2 years at 40°C (W/S = 0.4) (by I.G Richardson: The nature of C-S-H in hardened cements).\nFig. 2. A TEM micrograph that illustrates fine, dense Op C–S–H in the paste containing 75% slag. (by I.G Richardson: Composition and microstructure of 20-year-old ordinary Portland cement–ground granulated blast-furnace slag blends containing 0 to 100% slag).\nIn the case of C-S-H, its morphology and composition may be modified by partial accommodation of M and A within the micro- or nanostructure, its Ca/Si ratio is then lowered (e.g., 1.55) than that formed from alite and belite (e.g. 1.7). Hydrotalcite-like phase with approximate composition Mg6Al2(OH)16(CO3)·4H2O is formed from the MgO content of BFS, typically 5-9%.\nAs stated above, the hydration products can be classified into inner product and outer product. Inner product C-S-H from cement grains has a Ca/(Si+Al) ratio similar to outer product C-S-H, Meanwhile, Katoite (C3ASαHβ, α \u0026lt; 1.5) has also been suggested as a slag product, but it is less documented than the former mentioned species.\n","permalink":"https://www.cementscience.com/2012/06/hydration-products-of-slag-in-blended-cement.html","summary":"\u003cp\u003eMany XRD analysis results have shown the main hydration products of slag blended cement are essentially similar with that of pure Portland cement, except the amounts of CH found by this method or other are in varying degrees and less than those that should be given by the pure Portland cement constituent if the slag part did not participate the reaction.\u003c/p\u003e\n\u003cp\u003eThe main hydration products of the slag-cement are C-S-H gel, Ca(OH)\u003c!-- raw HTML omitted --\u003e2\u003c!-- raw HTML omitted --\u003e, the sulpho-aluminate hydrate phases AFt and AFm and a Mg, Al-rich hydroxide phase.\u003c/p\u003e","title":"Hydration products of slag in blended cement"},{"content":"The latent hydraulic property of slag means no hydration products could be observed when slag is solely placed in contact with water, though surface analysis using X-ray photoelectron spectrometry showed that the surface of slag was modified as soon as it came into contact with water making a protective film lacking Ca2+ that prevent further reaction, thus, slag dissolves to a small extent.\nThe hydration of slag and cement is more complex than that of Portland cement; given that both slag and cement take part in the reaction with water.\nThe glass network of slag is mainly the cause of its latently hydraulic properties. Adding activators slag could be activated to hydrate. There are two methods known to activate slag, viz. the addition of high amounts of calcium sulphate and alkali activation. The drawback of the former method requires long curing period and is sensitive to carbonation and frost attack, whilst the latter has excessive shrinkage and efflorescence as well as the intensive energy consumption in the production of alkaline activator.\nBlended with Portland cement, slag can be activated with a relatively high pH solution of blend system caused by the hydration phase CH, which is one of the main hydration products of C3S and C2S in Portland cement. slag has been successfully used with Portland cement to produce blended cements. As soon as water is added into the slag and Portland cement system, the latter begin to hydrate and a small amount of slag reacts as well due to the existence of gypsum in cement.\nAs the hydration of Portland cement proceeds, more and more alkali is available in the pore solution resulting in a high pH value (e.g. 13), which greatly activates the hydration of slag. Later, as the formation of CH proceeds due to the hydration of alite and belite, the hydration of slag is activated by CH, which results in microstructure development and strength gain of paste; however, the content of CH in the blended system increases initially and then decrease showing CH not only acts as an activator for the hydration of slag but a reactant.\nIt is noted that this method is only feasible with limited proportions of slag blended in cement. If very high proportion of slag is blended, the early strength may be markedly reduced, which is the major concern for application in the construction industry, and it is aggravated when a coarse slag is used.\nResearch conducted by F. Bellmann shows that activation is also possible by lowering the pH to a range between 11.8 and 12.2 by the addition of calcium hydroxide and soluble calcium salts which include calcium chloride, calcium bromide, calcium nitrate, calcium formate, and calcium acetate. By the mixture of the two additives, CH acts as reactant precipitating aluminium in an AFm phase, meanwhile, due to its presence, soluble calcium salts can decrease the pH value in pore solution as long as the equilibrium condition of calcium hydroxide is maintained.\n","permalink":"https://www.cementscience.com/2012/06/activation-of-slag-in-blended-cement.html","summary":"\u003cp\u003eThe latent hydraulic property of slag means no hydration products could be observed when slag is solely placed in contact with water, though surface analysis using X-ray photoelectron spectrometry showed that the surface of slag was modified as soon as it came into contact with water making a protective film lacking Ca\u003c!-- raw HTML omitted --\u003e2+\u003c!-- raw HTML omitted --\u003e that prevent further reaction, thus, slag dissolves to a small extent.\u003c/p\u003e","title":"Activation of slag in blended cement"},{"content":"The exact composition of slag varies over a range. In general, factors that determine the suitability of slag for usage in composite cement mainly include the fineness of grinding, glass content and the chemical composition.\nFineness Like most of other cement materials, the reactivity of slag is influenced by its surface area. Increased surface area leads to better strength development and more water requirement; however, the fineness of slag is limited from practical aspects, such as economic and performance considerations, setting time and shrinkage. The following table shows typical fineness data of market slag in some countries.\nTable: the surface area of slag in some countries (m2/Kg)\nUK USA Canada India Blaine surface area 375-425 450-550 450 350-450 Glass content During the quenching process, the liquid slag forms glassy and crystalline contents. Practical glass content of slag depends on the cooling rate, in general, rapid rate results in high glass content. The main difference between glass content and crystal content of slag is that the former part has a latent hydraulic property that makes the glass content of slag a very important factor affecting the engineering performance of slag cement.\nThough some researchers did obtain a roughly linear relationship between glass content and strength, there is no well-defined relationship between the glass content and strength of slag cement.\nAs for the relationship between hydraulicity and glass content, increasing glass content of slag improves its hydraulicity; however, research data that slag samples with 30-65% glass contents are still suitable has not shown exact correlation between them. Due to this uncertainty, most international standards classify slag reactivity by testing its direct strength rather than requiring minimum glass content. But from a practical standpoint, the glass content of slag should exceeds 90% to guarantee satisfactory properties.\nChemical composition As stated above, the chemical composition of slag is mainly the four components, namely, MgO, Al2O3, SiO2, and CaO. From a metallurgical standpoint, slag can be sorted as either basic or acidic, and the more basic of slag, the greater its hydraulic activity in the presence of alkaline activators, Lea also reported that the hydraulic values of slag increase with the increasing CaO/SiO2 ratio up to a limiting value (not precisely stated). Further, in European Standard EN 197-1:1992 and British Standards, the ratio of the mass MgO plus CaO to SiO2 must exceed 1.0, by which the high alkalinity is guaranteed and otherwise the slag would be hydraulically inactive.\nWith a constant CaO/SiO2 ratio, the strength of hydrated slag increases with the Al2O3 content, and a large amount of Al2O3 can compensate the deficiency of CaO. Further research, by a regression analysis of compressive strength on composition using a wide range of west European slags, showed that increase in Al2O3 content above 13% tended to increase the early strengths but to decrease late strengths. Moreover, the content of Al2O3 also influences the sulfate resistance of slag concrete.\nThe influence of MgO as a replacement of CaO seems depending on both the basicity and the MgO content of slag. Variations in the MgO content up to 8-10% may have little effect on strength development, but high content have an adverse effect. It also reported that MgO in amount up to 11% was quantitatively equivalent to CaO. Frearon and Higgins reported that to get a satisfactory sulfate resistance the content of MgO should be about 13%.\nMany researchers attempted to quantify the reactivity of slag considering the four major components together. Among these results, ratio (CaO+MgO+Al2O3)/SiO2 is the simplest and most widely used one. It was observed that the hydraulic activity of slags increases with the increasing contents of CaO, MgO and Al2O3 but decreases with the increasing content of SiO2. Furthermore, minimum values for this ratio, such as 1.0 (Germany) and 1.4 (Japan) have already been adopted in some countries’ standard specifications.\nApart from the four major components, there are also some minor components that may have important effect on the properties of slag, such as MnO is always negative, P2O5 and alkalis are more complicated.\n","permalink":"https://www.cementscience.com/2012/06/factors-affecting-the-reactivity-of-slag.html","summary":"\u003cp\u003eThe exact composition of slag varies over a range. In general, factors that determine the suitability of slag for usage in composite cement mainly include the fineness of grinding, glass content and the chemical composition.\u003c/p\u003e\n\u003cul\u003e\n\u003cli\u003e\u003cstrong\u003eFineness\u003c/strong\u003e\u003c/li\u003e\n\u003c/ul\u003e\n\u003cp\u003eLike most of other cement materials, the reactivity of slag is influenced by its surface area. Increased surface area leads to better strength development and more water requirement; however, the fineness of slag is limited from practical aspects, such as economic and performance considerations, setting time and shrinkage. The following table shows typical fineness data of market slag in some countries.\u003c/p\u003e","title":"Factors affecting the reactivity of slag"},{"content":"Though the chemical reaction of the fine particles of limestone in cement paste is limited to a low extent due to its inert property, the addition of limestone particles has significant effect on the microstructure development. Research conducted by Sellevold et al. using mercury intrusion method showed that specimens containing 12% CaCO3, which have the main body of the particles smaller than 0.1 µm had finer pore structure and somewhat reduced total pore volume.\nThey attribute this observation to the nucleation effect: The introduction of a large number of nucleation sites could result in a more homogeneous distribution of calcium silicate hydrate and thus a less open pore structure. The effect appears to be in the capillary pore structure rather than in the gel pores. The size and distribution of CH are also influenced by the presence of limestone.\nIn a limestone-filled paste which used 25% limestone larger regions of calcium hydroxide were unevenly distributed throughout paste while in the case of Portland cement small regions calcium hydroxide were evenly distributed. Further investigation found that limestone added in amounts of 5% or 25% enhance the formation of hydration rims of calcium silicate hydrate surrounding C3S particles due to the accelerated hydration rate of C3S.\nResults from the image analysis showed that the interface between limestone and hydrates in limestone-filled self-compacting concrete (SCC) is quite porous, while the interface around the unhydrated cement in high performance cement paste is much denser. Figures show a comparison of microstructure using BSE between limestone-filled cement paste and Portland cement paste. Two possible reasons could be responsible for this distinct difference in mcrostruture.\nOn the one hand, as the hydration process of cement proceeds, cement particles expand and get connect with each other to form a network, which result in strength gain; However, limestone particles do not expand during the whole hydration process due to its low reactivity, thus making the porosity of the former becomes lower than the latter one.\nOn the other hand, the addition of limestone may play a negative role in the microstructure development process, because it could block the expansion of hydrating cement, which makes the microstructure of limestone-filled cement paste more porous as showed in figure.\nComparison of BSE images of limestone cement (up) and Portland cement (down) at age of 7 days\nResearch by Pipilikaki et al. showed that limestone used in blended cements changes hardened cements’ pore structure. The capillaries pore size is increased from 20 nm to 40 nm when the maximum amount (35%) of limestone that is allowed by EN 197-1. At the same time, the addition of limestone reduces the threshold diameter of the paste and presents a more uniform pore size distribution.\nThe author concluded that this behavior can be attributed to the better packing of particles due to the filling effect of the limestone powder, resulting in that chemical species enter the hardened cement more difficult but transport easier inside the cement paste due to the pores have approximately the same size. As gel pores are concerned, addition of limestone in cement produces smaller gel pores probably due to the accelerated hydration rates.\n","permalink":"https://www.cementscience.com/2012/06/microstructure-development-of-limestone-blended-cement.html","summary":"\u003cp\u003eThough the chemical reaction of the fine particles of limestone in cement paste is limited to a low extent due to its inert property, the addition of limestone particles has significant effect on the microstructure development. Research conducted by Sellevold et al. using mercury intrusion method showed that specimens containing 12% CaCO\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003e, which have the main body of the particles smaller than 0.1 µm had finer pore structure and somewhat reduced total pore volume.\u003c/p\u003e","title":"Microstructure development of limestone blended cement"},{"content":"The extent of reaction of limestone with cement clinkers is relatively low than the corresponding values of cement clinkers, the probable cause for this as stated above arise from the low solubility and low reactivity of limestone particles, though other factors of limestone, including fineness, particle size distribution, etc., do have influence on its reaction degree in blended system.\nIn experiments of 5% or 15% calcium carbonate reaction with type II cement hydrated up to one year, Klemm and Adams observed that monocarbonate hydrate is formed slower than that of ettringite, and after 129 days hydration, the amount of unreacted CaCO3 is still up to 80-90%. Ramachandran investigated that in mixtures hydrated with 15% and 5% limestone substitution, the amounts of limestone reacted with the hydrating C3S were reacted within the first 3 days. A typical simulation performed by Bentz showed that for a 20% by mass fraction substitution of ground limestone for cement, only about 5% of the limestone present reacts during the first 180d of hydration.\nTaylor summarized that the maximum quantity of CaCO3 that can react appears to be 2-3% with most cements, and value up to 5.8% have also been reported; however, he did not mention the substitution level of limestone in cement. The relatively low reaction degree of limestone in blended cement is probably because of the low reactivity of limestone which is also the reason why limestone is regarded as inert “filler” by many researchers.\nIt is worth noting that the conclusion limestone being regarded as inert filler always arise from the fact high levels of limestone applied. At low substitution level, e.g. using up to 5% calcite, much or perhaps all of the added calcite is reactive with cement.\nIn terms of the quantitative relationship between the reactive fractions of limestone and time, it is still a challenge, no fundamental result is available from literature, not to mention limestone is considered as inert filler by many researchers provided that large amount of limestone is applied.\n","permalink":"https://www.cementscience.com/2012/06/low-reactivity-and-reported-reaction-extent-of-limestone-in-blended-cement.html","summary":"\u003cp\u003eThe extent of reaction of limestone with cement clinkers is relatively low than the corresponding values of cement clinkers, the probable cause for this as stated above arise from the low solubility and low reactivity of limestone particles, though other factors of limestone, including fineness, particle size distribution, etc., do have influence on its reaction degree in blended system.\u003c/p\u003e\n\u003cp\u003eIn experiments of 5% or 15% calcium carbonate reaction with type II cement hydrated up to one year, Klemm and Adams observed that monocarbonate hydrate is formed slower than that of ettringite, and after 129 days hydration, the amount of unreacted CaCO\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003e is still up to 80-90%. Ramachandran investigated that in mixtures hydrated with 15% and 5% limestone substitution, the amounts of limestone reacted with the hydrating C\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003eS were reacted within the first 3 days. A typical simulation performed by Bentz showed that for a 20% by mass fraction substitution of ground limestone for cement, only about 5% of the limestone present reacts during the first 180d of hydration.\u003c/p\u003e","title":"Low reactivity and reported reaction extent of limestone in blended cement"},{"content":"The hydration rate of C3S is accelerated in the presence of limestone probably because of the dilute effect and the multiplied nucleation sites. Jean Pera et al. reported that the total heat resulting from pure C3S hydration was 145 joules while that of the mixture (50%C3S+50%CaCO3) reached 260 joules. Ramachandran’s investigation showed that some calcium carbonate was consumed as the hydration of Portland cement proceeded. The product of the reaction of limestone and C3S is calcium carbosilicate, whose exact type cannot be identified by X-ray diffraction probably due to its amorphous property and small amount of formation.\nBesides the reaction with C3S, limestone can reacts with C3A as well. According the investigation of Ingram et al., for a combination of 2% gypsum, 6% limestone, and 92% clinker, CaCO3 reacts with C3A in the clinker. The reaction begins with a C3A·CaCO3·12H2O product, then forms compounds containing a molar ratio of C3A to CaCO3 between 0.5 and 0.25. Later, the product appears to stabilize as C3A·xCaCO3·11H2O, where x ranges from 0.5 to 0.25. Other researchers reported similar results.\nBensted found that in the absence of gypsum CaCO3 in limestone reacts with C3A to form both \u0026ldquo;hexagonal prism\u0026rdquo; phase tricarbonate C3A·3CaCO3·30H2O and hexagonal plate phase monocarbonate C3A·CaCO3·11H2O, but the former one tricarbonate is much less stable than AFt at ambient temperature, thus it would not be formed in cement hydration.\nThe transformation of ettringite to monosulfate in the presence of limestone is delayed and reduced due to the formation of monocarboaluminate. Bentz proposed a possible chemical reaction of this process as follows,\n3(CaO)3(Al2O3)·CaSO4·12H2O+2CaCO3 +18H2O → 2(CaO)3(Al2O3)·CaCO3·11H2O + (CaO)3(Al2O3)·3CaSO4·32H2O\nG. Kakali et al. concluded that in pastes containing CaCO3, either as a chemical reagent or as a limestone constituent, the ettringite’s transformation to monosulfate is delayed, while calcium aluminate monocarbonate is preferably formed instead of monosulfate even at early ages.\nIt is should be noted that the formation of ettringite is accelerated by the addition of limestone at the very beginning of hydration (e.g. 30 min) in the presence of gypsum, corresponding with the accelerated conversion of ettringite to monosulphoaluminate due to the incorporation of limestone.\n","permalink":"https://www.cementscience.com/2012/06/chemical-reaction-of-limestone-with-c3s-and-c3a.html","summary":"\u003cp\u003eThe hydration rate of C\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003eS is accelerated in the presence of limestone probably because of the dilute effect and the multiplied nucleation sites. Jean Pera et al. reported that the total heat resulting from pure C\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003eS hydration was 145 joules while that of the mixture (50%C\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003eS+50%CaCO\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003e) reached 260 joules. Ramachandran’s investigation showed that some calcium carbonate was consumed as the hydration of Portland cement proceeded. The product of the reaction of limestone and C\u003c!-- raw HTML omitted --\u003e3\u003c!-- raw HTML omitted --\u003eS is calcium carbosilicate, whose exact type cannot be identified by X-ray diffraction probably due to its amorphous property and small amount of formation.\u003c/p\u003e","title":"Chemical reaction of limestone with C3S and C3A"},{"content":"Effects of limestone addition on the hydration of limestone blended cement can be classified into two aspects, viz. physical effects and chemical effects.\nNumerous researchers who investigated Portland limestone cement with high level of calcite addition regard it as inert filler, e. g. by means of both thermal and BSE image analysis, it was investigated by G. Ye et al. that limestone powder does not take part in the chemical reaction at all.\nThe low reactivity of limestone due to its low solubility is the main cause leading to the inert property; however, even acting as filler, limestone in blended cement causes an apparent hydration acceleration of cement clinker especially at early ages.\nOn the one hand, the effective w/c ratio in limestone blended system is increased significantly due to the low reactivity of limestone powder, altering the hydration characteristics of cements and providing more water and space for the hydration of clinkers.\nOn the other hand, limestone is softer than clinker which could achieve a finer particle size when interground with Portland cement clinkers, producing an improved particle size distribution and improving particle packing, e.g., for an overall specific Blaine surface area of 420 m2/ kg, 50% of the limestone particles can be below 700nm, compared with 3µm for the clinkers;\nTherefore, a large number of tiny limestone particles act as nucleation sites for the hydration of C3S (and also C2S ), which then markedly decrease the concentration of Ca and Si ions in the solution phases promoting the transformation of C3S phase to the solution phase, thus the hydration of C3S being accelerated.\n","permalink":"https://www.cementscience.com/2012/06/physical-effects-of-limestone-on-the-hydration-of-cement-clinkers.html","summary":"\u003cp\u003eEffects of limestone addition on the hydration of limestone blended cement can be classified into two aspects, viz. physical effects and chemical effects.\u003c/p\u003e\n\u003cp\u003eNumerous researchers who investigated Portland limestone cement with high level of calcite addition regard it as inert filler, e. g. by means of both thermal and BSE image analysis, it was investigated by G. Ye et al. that limestone powder does not take part in the chemical reaction at all.\u003c/p\u003e","title":"Physical effects of limestone on the hydration of cement clinkers"},{"content":"The binary cement, e.g. Portland cement blends with slag or fly ash or limestone, has gained great popularity in many countries. However, each kind of binary cement has its own shortfalls, e.g. the addition limestone can reduce the later strength due to its dilution effect, while the reaction of slag is relatively slow in the early ages.\nTo utilize materials more effectively and reduce the cost in construction industry, ternary cement that made with Portland clinkers and other two admixtures may be a better option because it presents several advantages over binary cements. With the development of separate grinding and mixing technology in cement industry, it is becoming more convenient to produce these so-called market-oriented or tailor-made cements.\nThe combination of limestone and slag with Portland cement can help to produce a new cement-based material which has advantage over binary blended cement. An obvious advantage is that limestone contributes to the early strength while slag increases the long-term strength, this leads to an adequate development of strength compared with either slag cement or limestone cement.\nTo find the strength development of ternary cement with limestone filler and blast-furnace slag, Menendez et al. tested mortar prisms in which Portland cement was replaced by up to 20% limestone and 35% blast-furnace slag. The test at 1, 3, 7, 28 and 90 days shows that the contribution of limestone to the hydration degree of Portland cement at 1 and 3 days increases the early strength of ternary system containing about 5-15% limestone and 0-20% blast-furnace slag. The later hydration of blast-furnace slag is very effective in producing ternary cements with similar or higher compressive strength than Portland cement at the ages of 28 days and 90 days.\n","permalink":"https://www.cementscience.com/2012/05/advantage-of-ternary-blended-cement.html","summary":"\u003cp\u003eThe binary cement, e.g. Portland cement blends with slag or fly ash or limestone, has gained great popularity in many countries. However, each kind of binary cement has its own shortfalls, e.g. the addition limestone can reduce the later strength due to its dilution effect, while the reaction of slag is relatively slow in the early ages.\u003c/p\u003e\n\u003cp\u003eTo utilize materials more effectively and reduce the cost in construction industry, ternary cement that made with Portland clinkers and other two admixtures may be a better option because it presents several advantages over binary cements. With the development of separate grinding and mixing technology in cement industry, it is becoming more convenient to produce these so-called market-oriented or tailor-made cements.\u003c/p\u003e","title":"Advantage of ternary blended cement"},{"content":"In the late 1980s, Johnson and Jennings wrote a program which was based on the idea that cement hydration is considered as nucleation and growth of spherical particles in three-dimensional space.\nHYMOSTRUC was built by K. van Breugel, this model is based on the assumption that the growth of new layers of hydration products is deposited on the surface of cements particles (mostly alite particles considered), which leads to a more heterogeneous distribution of hydration products. The hydrating cement particles are represented as expanding spheres. At the contact zone, where two hydrating cement particles meet, the overlapping volume of hydration products is redistributed around the two touching particles. The model can simulate the development of properties of Portland cement, e.g. the development of hydration and microstructure, the volume changes of the hardening cement pastes, and the effect of geometrical changes of the microstructure on the creep of the hardening concrete. The emphasis of the model is on the formation of the microstructure and the corresponding bulk properties, while the evolution of hydrating product phases is less focused.\nBased on HYMOSTRUC model, Liu Xian et al. made an improvement to take account of the addition of limestone into Portland cement. Due to large substitution level (say 33% and 42%) of Portland cement, limestone particles are considered as no-expanding particles and inert filler without taking part in the hydration process.\nTo better represent the accurate microstructure of hardening Portland cement, Integrated Particle Kinetics Model (IPKM) was developed, the assumption of IPKM is that the evolution of alite hydration is modeled by the deposition of C-S-H on the surface of C3S particles but the formation of new portlandite is assumed to take place in pores, which is not considered in HYMOSTRUC; therefore, it is possible to enable the calculation of interaction between particles and evolution of individual particles, thus enabling the modeling of the evolution of each particle independently. However, due to the explicit calculation of all possible interactions, the simulations using IPKM is very slow, which leads to the simulations only within relatively small number of particles.\nSimilar to IPKM, a new platform for modeling the hydration of cements called µic is developed, which is claimed to have improved the performance of the continuous approach enabling simulations with millions of particles within acceptable times compared with IPKM. Besides the high calculation efficiency, the application enables the customization of all aspects of microstructural development of hardening cement paste.\nOne of the best known models using discretization approach is called CEMHYD3D which was launched by Garboczi and Bentz. The model is used to simulate the development of properties of cement-based materials, e.g. the microtructure development of hardening cement paste, the adiabatic temperature rise of Portland cement and silica fume blended concrete, and the diffusivity of chloride ions in silica fume blended cement paste. The features of this model are digital image basis, accurate microstructure representation, and rule-based to mimic reaction and diffusion. The drawback is that there is little or no kinetic information corresponding to the hydration process and requiring magic resolution which substantially increases the computation time of a relatively large volume cement paste. As for binary cement, preliminary work were tried to incorporate the reaction of fly ash and slag; however, due to the complexity of the reaction of slag blended cement, more effort is needed for this model to deal with the reaction kinetic constant and activation energy of fly ash and slag, meanwhile, the induction period of slag or fly ash blended cement is not explicitly considered in the model limiting the application of the model in predicting the properties of early-age concrete.\nOriginally based on the CEMHYD3D, Chen Wei extended the model to simulate the hydration and microstructure development of slag cement. Some modifications were made to consolidate the chemical background of the model and eliminate the effect of system resolution on the model predictions, especially the hydration degree of cement. The model can be used to investigate the various stages of cement hydration. As the author stated, the new version model has its own drawbacks, such as the reactivity of slag has not been taken into account adequately, the role of activator is constrained only to the activation from Portland cement/clinker.\nMaekawa et al. proposed an integrated program named DUCOM (DUrability COncrete Model), which evaluates both the early-age properties of hardening concrete (such as the cement heat hydration and thermal conduction, pore structure formation and moisture equilibrium) and durability of concrete (e.g. chloride ion transport, carbonation, corrosion of steel re-bar and calcium ion leaching). The old version DUCOM model can be used to evaluate the temperature history of slag or fly ash blended concrete. In the latest updated DUCOM model, the effect of limestone powder and the reaction of silica fume are incorporated. However, DUCOM model did not consider too much on the chemical aspects of the hydration of binary cements. The influence of mineral compositions of fly ash or silica fume on reaction stoichiometry is not considered in DUCOM model yet. The evolution of chemical and volumetric composition of silica fume-cement blends or fly ash cement blends cannot be evaluated.\nG. De Schutter proposed a kinetic hydration model which is valid for Portland cement and blast furnace slag cement. In his model, the heat evolution of blast furnace slag cement is obtained by the superposition of the heat release of the Portland reaction (P reaction) and the slag reaction (S reaction). The evolution of mechanical properties in early-age concrete is described using functions of the degree of hydration. However, the interactions between the cement hydration and the reaction of mineral admixtures, e.g. the production of calcium hydroxide by cement hydration and the consumption calcium of hydroxide by slag reaction, are not considered in the hydration model yet. On the other hand, The generalization of the reaction parameters depending on the actual slag replacement ratios is not yet possible.\nConsidering the production of portlandite from cement hydration and the consumption in the reaction of mineral admixtures, a numerical hydration model is recently developed by Wang et al. In this model, the heat evolution rate of fly ash- or slag-blended concrete is determined by the contribution of both cement hydration and the reaction of mineral admixtures, where the total heat generation content of fly ash and slag is set as 110 kcal/kg and 50 kcal/kg, respectively. With regards to CH, it is assumed the amount of CH is directly proportional to the degree of hydration of cement, and the reaction of slag is accelerated by the presence of CH and be dependent on the mass of CH. Using this model, the prediction of temperature rise from modeling results in blended cement agrees well with the experimental results, as well as the temperature distribution in blended cement is predicted. However, influence of the chemical compositions of admixtures on the reaction stoichiometry of admixture is not taken account for in the model, and hydration product phase’s distribution and microstructure development are not included in the model.\n","permalink":"https://www.cementscience.com/2012/05/review-of-several-existing-models-simulating-the-hydration-of-cementitious-materials.html","summary":"\u003cp\u003eIn the late 1980s, Johnson and Jennings wrote a program which was based on the idea that cement hydration is considered as nucleation and growth of spherical particles in three-dimensional space.\u003c/p\u003e\n\u003cp\u003eHYMOSTRUC was built by K. van Breugel, this model is based on the assumption that the growth of new layers of hydration products is deposited on the surface of cements particles (mostly alite particles considered), which leads to a more heterogeneous distribution of hydration products. The hydrating cement particles are represented as expanding spheres. At the contact zone, where two hydrating cement particles meet, the overlapping volume of hydration products is redistributed around the two touching particles. The model can simulate the development of properties of Portland cement, e.g. the development of hydration and microstructure, the volume changes of the hardening cement pastes, and the effect of geometrical changes of the microstructure on the creep of the hardening concrete. The emphasis of the model is on the formation of the microstructure and the corresponding bulk properties, while the evolution of hydrating product phases is less focused.\u003c/p\u003e","title":"Review of several existing models simulating the hydration of cementitious materials"},{"content":"With the development of computer technology, increasing attention is being paid to the modeling work of cementitious-based materials. Many researchers have been carrying out the research to better model the hydration of cement-based materials in the last decades. It is obvious that a cogent simulation of the hydration of cement-based materials has crucial role in construction industry, such as reducing tedious process of trial and error when doing experiments, facilitating the research of durability of concrete.\nMany models are available to model the hydration process and microstructure of cement-based materials. According the simplifications of hydration models, two main approaches could be classified, viz. continuous approach and discretization approach. Because of the complexity of real hardening cement-based materials, each model is based on certain assumptions that aim to simplify the complexity of real cement microstructure and its interactions.\nHYMOSTRUC (by TuDelft)\nThe advantages of continuous approach are resolution free and no requirement to divide features of microstructure into smaller elements. Particles are normally assumed as sphere shapes. The assumption of sphere demands less information to describe particles when modeling compared with other shapes, thus resulting in the calculation of the distance between two particles fast. This method also preserves information about features that scale over several orders of magnitude, viz. from micrometers to millimeters. However, the drawback of this method is that the geometry of microstructure is altered.\nCEMHYD3D (by NIST, USA)\nThe principle of discretization approach is similar to finite element method. The entire volume of the microstructure is filled with smaller elements which are placed with their faces in contact. By means of a certain algorithm, the hydration and microstructure development of cement could be simulated.\n","permalink":"https://www.cementscience.com/2012/05/two-main-methods-to-model-cement-based-materials.html","summary":"\u003cp\u003eWith the development of computer technology, increasing attention is being paid to the modeling work of cementitious-based materials. Many researchers have been carrying out the research to better model the hydration of cement-based materials in the last decades. It is obvious that a cogent simulation of the hydration of cement-based materials has crucial role in construction industry, such as reducing tedious process of trial and error when doing experiments, facilitating the research of durability of concrete.\u003c/p\u003e","title":"Two main methods to model cement-based materials"},{"content":"Limestone has been utilized as a mineral addition in cement industry for a long time. The latest European Standard (EN 197-1-2000) allows up to 5% limestone as a minor additional constituent, and also identifies four types of Portland limestone cement containing 6-20% limestone (types II/A-L and II/A-LL) and 21-35% limestone (types II/B-L and II/B-LL), respectively. The ASTM Standard (C150-04) allows up to 5% of limestone filler. Since the early 1980s, the Canadian cement standard has allowed the inclusion of up to 5% limestone addition to Portland limestone cement.\nSimilar trend could also be found in Latin-American countries such as Argentina, Brazil, and Mexico (Menendez). According the review Cement Standards of the World (CEMBUR-EAU 1997), more than 25 countries allow the use of between 1% and 5% limestone in their Portland cement. Many countries even allow up to 35% replacement in Portland composite.\nCompositions analysis of several typical limestone\nThe main composition of limestone is calcite (CaCO3), with smaller proportion of quartz or amorphous silica and sometimes of dolomite. Table above is composition analysis of several typical limestones. Though the LOI content of limestone is up to 42.5% or even more, they must be low in clay minerals and organic matter to guarantee the water demand and setting time. As for the quality requirement, according to ASTM Standard (ASTM C-150-4), the calcium carbonate (CaCO3) content calculated from the calcium oxide content should be at least 70% by mass.\nLimestone is softer than cement clinkers, thus could be grind into finer particles. When it interground with clinkers, for an overall specific surface area (Blaine) of 420 m2/kg, 50% of the limestone can be below 700nm, compared with 3 µm for the corresponding clinker. Addition of finer limestone particles to clinker completes the fine fraction in the granulometric curve of cement without an increment on water demand, and improves the cement packing and blocks the capillary pores.\n","permalink":"https://www.cementscience.com/2012/05/brief-introduction-of-limestone-cement.html","summary":"\u003cp\u003eLimestone has been utilized as a mineral addition in cement industry for a long time. The latest European Standard (EN 197-1-2000) allows up to 5% limestone as a minor additional constituent, and also identifies four types of Portland limestone cement containing 6-20% limestone (types II/A-L and II/A-LL) and 21-35% limestone (types II/B-L and II/B-LL), respectively. The ASTM Standard (C150-04) allows up to 5% of limestone filler. Since the early 1980s, the Canadian cement standard has allowed the inclusion of up to 5% limestone addition to Portland limestone cement.\u003c/p\u003e","title":"Brief introduction of limestone cement"},{"content":"Blast-furnace slag (BFS) is formed from a liquid at 1350-1550 °C during the manufacture of iron. When reaching the bottom of the furnace, the liquid slag forms a layer on top of the molten iron due to its lower density. Being separated from the molten iron, the liquid slag is cooled in the air or with water. Depending on the way of cool process, three main categories of BFS could be produced, which are namely ground granulated BFS, pelletized slag and air-cooled slag.\nGround granulated blast-furnace slag (GGBFS), which normally contains up to 95% of glass, is formed by cooling the liquid slag with large amount of water and subsequently ground to fine powder.\nIf the liquid slag is partially cooled with water and then flung to air, pelletized slag could be thus produced. Comparing with GGBFS, pelletized slag contains much low glass content, e.g. 50%, therefore it is normally used as concrete aggregate or as raw materials to produce cement clinkers.\nWhen cooled and solidified in the air, air-cooled slag is produced. During the production process, a water spray procedure is sometimes applied to accelerate the cooling process. Because of the hard and dense property, air-cooled slag is utilized in road bases, asphalt paving or as concrete aggregate, etc.\nAmong these three kinds of slag, GGBFS is the most valuable one in cement industry. Due to its cementitious properties mixing with lime, alkalis or Portland cement, GGBFS is often used to make blast-furnace slag cement. The history of the production of slag cement in Germany, France, Luxembourg and Belgium has been more than one century.\nThe usage of slag cement, which based on partial replacement of Portland cement by slag, has mainly three advantages. First, it offer cost reduction because blast-furnace slag is a byproduct of steel industry, which makes it cheaper than Portland cement on the one hand, though the increasing demand increases the market price more or less; on the other hand, utilization of byproducts from steel industry also protects environment. Second, the manufacture of slag cement requires 75% less energy than that needed for the production of Portland cement. The less energy demand brings environmental benefit, cost save, and less emission of carbon dioxide that causes the planet warmer. Third, the use of slag cement can arguably improve the properties of cement products, e.g. better concrete workability, lower permeability, improved resistance to aggressive chemicals, higher compressive and flexural strengths, etc.\n","permalink":"https://www.cementscience.com/2012/05/introduction-slag-cement.html","summary":"\u003cp\u003eBlast-furnace slag (BFS) is formed from a liquid at 1350-1550 °C during the manufacture of iron. When reaching the bottom of the furnace, the liquid slag forms a layer on top of the molten iron due to its lower density. Being separated from the molten iron, the liquid slag is cooled in the air or with water. Depending on the way of cool process, three main categories of BFS could be produced, which are namely ground granulated BFS, pelletized slag and air-cooled slag.\u003c/p\u003e","title":"Introduction of slag cement"},{"content":"Twitter | Facebook\nWhat is CementScience.com?\nwww.CementScience.com is a blog created by Zhijun Tan on research of Cement Science. It is a world of Cementitious Materials. Welcome to visit the website.\nWho am I?\nMy name is TAN Zhijun. I come from Hunan province of southern China. I obtained my PhD from the Faculty of Engineering and Architecture of Ghent University, Belgium. My doctoral research topic focused on the hydration modeling of cement-based materials which is made of ternary blended Portland cement, blast-furnace slag and limestone powder.\nI am now working at the University of Sheffield, the United Kingdom, with research topics focusing on the hydration modeling of cement-based materials and sustainable construction materials, i.e. blended cement and geopolymer concrete.\n","permalink":"https://www.cementscience.com/about/","summary":"\u003cp\u003e\u003ca href=\"https://twitter.com/tumutanzi\"\u003eTwitter\u003c/a\u003e | \u003ca href=\"https://www.facebook.com/tumutanzi\"\u003eFacebook\u003c/a\u003e\u003c/p\u003e\n\u003cp\u003e\u003cimg alt=\"Cement Science\" loading=\"lazy\" src=\"/wp-content/uploads/2012/05/cement-science.png\"\u003e\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003eWhat is CementScience.com?\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003e\u003ca href=\"https://www.cementscience.com/\"\u003ewww.CementScience.com\u003c/a\u003e is a blog created by \u003ca href=\"https://www.tanzhijun.com/\"\u003eZhijun Tan\u003c/a\u003e on research of Cement Science. It is a world of Cementitious Materials. Welcome to visit the website.\u003c/p\u003e\n\u003cp\u003e\u003cstrong\u003eWho am I?\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eMy name is TAN Zhijun. I come from Hunan province of southern China. I obtained my PhD from the Faculty of Engineering and Architecture of Ghent University, Belgium. My doctoral research topic focused on \u003ca href=\"/Experimental-Study-and-Numerical-Simulation-of-Hydrationand-Microstructure-Development-of-Ternary-Cement-Based-Materials-UGent-Public-Doctoral-Thesis-Final-Version-Zhijun-Tan.pdf\"\u003ethe hydration modeling of cement-based materials\u003c/a\u003e which is made of ternary blended Portland cement, blast-furnace slag and limestone powder.\u003c/p\u003e","title":"About"},{"content":"Welcome to the world of cement www.CementScience.com, a brand new website with everything all about the science of cementitious materials.\nCement is a kind of important material for the modern construction industry. The most use of cement is for the making of concrete that is a magic artificial \u0026ldquo;stone\u0026rdquo; formed from the soft paste with aggregate. However, do you know what is behind the magic material?\nI am a PhD student who is the owner of this website, and works on the research of cement-based material. More precisely, the target of my research is Portland cement blended with blast-furnace slag and limestone powder. The research aims to get a more environment friendly cement with acceptable engineering performance.\nBesides my research, I would like to share some information with the people who are interested in cementitous material. This website is a world of cemetitous materials, with everything here on cementitious materials, such as cement, blended cement.\nYou are welcome to leave your comment on this site. I hope you also get some interesting information on cement, and even more.\n","permalink":"https://www.cementscience.com/2012/05/welcome-to-the-world-of-cementitious-materials.html","summary":"\u003cp\u003eWelcome to the world of cement \u003ca href=\"http://www.CementScience.com\"\u003ewww.CementScience.com\u003c/a\u003e, a brand new website with everything all about the science of cementitious materials.\u003c/p\u003e\n\u003cp\u003eCement is a kind of important material for the modern construction industry. The most use of cement is for the making of concrete that is a magic artificial \u0026ldquo;stone\u0026rdquo; formed from the soft paste with aggregate. However, do you know what is behind the magic material?\u003c/p\u003e\n\u003cp\u003eI am a PhD student who is the owner of this website, and works on the research of cement-based material. More precisely, the target of my research is Portland cement blended with blast-furnace slag and limestone powder. The research aims to get a more environment friendly cement with acceptable engineering performance.\u003c/p\u003e","title":"Welcome to the world of cementitious materials"}]